Docol® 800CP complex phase

Download data sheet

General Product Description

Docol 800CP is intended for designs where high structural strength and energy absorption are desired, suitable for cold formed safety components and crash-relevant equipment within the automotive and transport industries.

Dimension Range

Cold rolled / UC: thickness 0.50-2.10 mm, width up to 1527 mm.

Cold rolled / GI, GA, ZA: thickness 0.80-2.50 mm, width up to 1460 mm.

Hot rolled / UC: thickness 2.00-4.00 mm, width up to 1500 mm.

Hot rolled / GI: thickness 2.00-3.50 mm, width up to 1400 mm.

Slit strip and cut to length sheets are available upon request.

Grade and coating specific restrictions on available dimensions may occur.

Mechanical Properties

Docol CR​570Y​780T-​CP

Standard
VDA 239-100
Coating
UC, GI, GA*, ZA*
Test direction
L
Yield strength Rp0.2
(MPa)
570 - 720
Tensile strength Rm
(MPa)
780 - 920
Elongation A80
(min %)
10 1)
Elongation A5
(min %)
—
BH2
(min MPa)
30
Hole expansion ratio 2)
(min %)
—
Hole expansion ratio 2)
(% typical)
—

Docol HR​660Y​760T-​CP

Standard
VDA 239-100
Coating
UC, GI
Test direction
L
Yield strength Rp0.2
(MPa)
660 - 820
Tensile strength Rm
(MPa)
760 - 960
Elongation A80
(min %)
10
Elongation A5
(min %)
13
BH2
(min MPa)
30
Hole expansion ratio 2)
(min %)
—
Hole expansion ratio 2)
(% typical)
—

Docol HR800HER-75

Standard
SSAB
Coating
UC, GI
Test direction
L
Yield strength Rp0.2
(MPa)
660 - 820
Tensile strength Rm
(MPa)
760 - 960
Elongation A80
(min %)
11
Elongation A5
(min %)
14
BH2
(min MPa)
30
Hole expansion ratio 2)
(min %)
45
Hole expansion ratio 2)
(% typical)
75

Docol Roll 800

Standard
SSAB
Coating
UC
Test direction
T
Yield strength Rp0.2
(MPa)
600 - 750
Tensile strength Rm
(MPa)
800 - 950
Elongation A80
(min %)
10
Elongation A5
(min %)
—
BH2
(min MPa)
—
Hole expansion ratio 2)
(min %)
—
Hole expansion ratio 2)
(% typical)
—

*Available upon request.

1) For GA coatings the minimum elongation value is reduced by 2 units.

2) HER –ratio is average of three test results out of five tested samples by excluding minimum and maximum results.

Chemical Composition (ladle analysis)

Docol CR​570Y​780T-​CP

Coating
UC, GI, GA*, ZA*
C
(max %)
0.18
Si
(max %)
1.00
Mn
(max %)
2.50
P
(max %)
0.050
S
(max %)
0.010
Al
(%)
0.015 - 1.00
Nb+Ti
(max %)
0.15
Cr+Mo
(max %)
1.00
B
(max %)
0.005
Cu
(max %)
0.20

Docol HR​660Y​760T-​CP

Coating
UC, GI
C
(max %)
0.18
Si
(max %)
1.00
Mn
(max %)
2.20
P
(max %)
0.050
S
(max %)
0.010
Al
(%)
0.015 - 1.2
Nb+Ti
(max %)
0.25
Cr+Mo
(max %)
1.00
B
(max %)
0.005
Cu
(max %)
0.20

Docol HR800HER-75

Coating
UC, GI
C
(max %)
0.18
Si
(max %)
1.00
Mn
(max %)
2.20
P
(max %)
0.050
S
(max %)
0.010
Al
(%)
0.015 - 1.2
Nb+Ti
(max %)
0.25
Cr+Mo
(max %)
1.00
B
(max %)
0.005
Cu
(max %)
0.20

Docol Roll 800

Coating
UC
C
(max %)
0.16
Si
(max %)
0.40
Mn
(max %)
1.80
P
(max %)
0.020
S
(max %)
0.010
Al
(%)
From 0.015
Nb+Ti
(max %)
0.10
Cr+Mo
(max %)
—
B
(max %)
—
Cu
(max %)
—
* Available upon request.

Tolerances

Cold rolled (UC): Tolerances in accordance to EN 10131.

Hot rolled (UC): Tolerances in accordance to EN 10051.

Hot-dip galvanized (GI, GA, ZA): Tolerances in accordance to EN 10143.

Customized dimensional and shape tolerances are available upon request.

Coatings

The metal coating options for Docol® products include:

Hot-dip zinc coating (GI) consists almost entirely of zinc (>99%). It is lead free, resulting in a small zinc spangle size. The coating provides good corrosion protection.

Galvannealed coating (GA) is a zinc-iron alloy coating having an iron content of approximately 10%. Galvannealed is produced by post-heat treatment in continuous hot-dip coating process. Galvannealed provides excellent resistance weldability and corrosion protection of painted products.

Galfan coating (ZA) is a zinc-aluminium alloy coating having the eutectic composition approximately of 95% Zn and 5% Al. Galfan is produced in continuous hot-dip coating process. Galfan has better anticorrosive and forming properties than conventional hot-dip zinc coating (GI).

Electrogalvanized coating (EG) is applied continuously by electro deposition. The coating consists of zinc (>99%). Electrogalvanized steel is characterized by its excellent surface quality and uniform coating thickness.

Grade specific availability of metal coatings for Docol® products is given in the Mechanical properties table (Coating).

Coating type
Coating type
GI
Coating class
40/40
Standard
VDA 239-100
Closest in EN 10346, informative
Z100
Coating mass per side, single spot test (g/m2)
40 - 60 1)
Thickness per side informative (µm)
5.6 - 8.5
Coating type
Coating type
GI
Coating class
50/50
Standard
VDA 239-100
Closest in EN 10346, informative
—
Coating mass per side, single spot test (g/m2)
50 - 70 1)
Thickness per side informative (µm)
7.0 - 9.9
Coating type
Coating type
GI
Coating class
60/60
Standard
VDA 239-100
Closest in EN 10346, informative
Z140
Coating mass per side, single spot test (g/m2)
60 - 90
Thickness per side informative (µm)
8.5 - 12.7
Coating type
Coating type
GI
Coating class
70/70
Standard
VDA 239-100
Closest in EN 10346, informative
—
Coating mass per side, single spot test (g/m2)
70 - 100
Thickness per side informative (µm)
9.9 - 14.1
Coating type
Coating type
GI
Coating class
85/85
Standard
VDA 239-100
Closest in EN 10346, informative
—
Coating mass per side, single spot test (g/m2)
85 - 115
Thickness per side informative (µm)
12.0 - 16.2
Coating type
Coating type
GI
Coating class
115/115
Standard
VDA 239-100
Closest in EN 10346, informative
Z275
Coating mass per side, single spot test (g/m2)
115 - 155
Thickness per side informative (µm)
16.2 - 21.8
Coating type
Coating type
GA
Coating class
40/40
Standard
VDA 239-100
Closest in EN 10346, informative
ZF100
Coating mass per side, single spot test (g/m2)
40 - 60 1)
Thickness per side informative (µm)
5.6 - 8.5
Coating type
Coating type
GA
Coating class
50/50
Standard
VDA 239-100
Closest in EN 10346, informative
ZF120
Coating mass per side, single spot test (g/m2)
50 - 80
Thickness per side informative (µm)
7.0 - 11.3
Coating type
Coating type
ZA
Coating class
95
Standard
EN 10346
Closest in EN 10346, informative
ZA95
Coating mass per side, single spot test (g/m2)
—
Thickness per side informative (µm)
7.0 -
Coating type
Coating type
ZA
Coating class
130
Standard
EN 10346
Closest in EN 10346, informative
ZA130
Coating mass per side, single spot test (g/m2)
—
Thickness per side informative (µm)
10.0 -
Coating type
Coating type
EG
Coating class
25/25
Standard
EN 10152
Closest in EN 10346, informative
—
Coating mass per side, single spot test (g/m2)
12 -
Thickness per side informative (µm)
1.7 -
Coating type
Coating type
EG
Coating class
50/50
Standard
EN 10152
Closest in EN 10346, informative
—
Coating mass per side, single spot test (g/m2)
29 -
Thickness per side informative (µm)
4.1 -
Coating type
Coating type
EG
Coating class
75/75
Standard
EN 10152
Closest in EN 10346, informative
—
Coating mass per side, single spot test (g/m2)
47 -
Thickness per side informative (µm)
6.6 -
Coating type
Coating type
EG
Coating class
100/100
Standard
EN 10152
Closest in EN 10346, informative
—
Coating mass per side, single spot test (g/m2)
65 -
Thickness per side informative (µm)
9.1 -

Docol® metal coated products are available with surface quality for unexposed applications.

In addition to these coating masses, OEM specific coatings and single sided EG coatings are available upon request.

1) For hot-dipped (GI, ZA, GA) hot rolled (HR) grades, the coating mass tolerance is increased to 30 g/m² by increasing the upper limit.

Surface Treatments

Uncoated (UC): available as oiled.

Hot-dip galvanized (GI, GA, ZA): available as oiled and/or chemically passivated.

Electrogalvanized (EG): available as oiled and/or chemically passivated or phosphated.

All surface treatments are in accordance with RoHS directive (2011/65/EU) and do not contain Chromium VI (Cr6+). Surface treatments provide only temporary surface protection during transportation and storage. In order to avoid corrosion damages, care must be taken to keep the products dry during transportation and storage. If they become wet, they must be separated and situated so that they are dried quickly.

Fabrication and Other Recommendations

For information concerning fabrication, see SSAB´s brochures on www.ssab.com or consult Tech Support.

Appropriate health and safety precautions must be taken when bending, welding, cutting, grinding or otherwise working on the products.

Docol® Complex Phase steel product offer

Docol® 600 CP complex phase

Visa produkten

Docol® 800CP complex phase

Visa produkten

Docol® 1000CP complex phase

Visa produkten

Docol® 1200CP complex phase

Visa produkten

Relaterat innehåll

AHSS provplåtslager

Vill du upptäcka unika biltillämpningar, prova nya produktionsmetoder eller skapa lättare komponenter som ger bättre bränsleeffektivitet, krockprestanda och hållbarhet?

Läs mer

Formningsdata för Docol® AHSS-stål

Befintliga Docol® kunder får tillgång till formningsdata dygnet runt för att underlätta deras val och simulering av avancerat höghållfast fordonsstål.