Docol® Tube 590DP

Download data sheet

Select Language

Get datasheet by email
Close

Get datasheet by email

På denna sida

General Product Description

Docol®Tube 590DP is high-strength formable precision tube made from dual-phase steel with high tensile strength and very good formability. Available in circular, rectangular and square shapes, it comes with different coating and surface options including cold rolled (uncoated), galvanized, galvannealed and galfan. Customized shapes and other tailoring options are available upon request. Typically used in automotive industry where durability, formability and energy absorption are important.

Dimension Range

Docol Tube 590DP is available in circular, square and rectangular shapes.

Hide/Show specific columns Edit
Select columns to display
    Shapes Dimensions
    Circular (mmin) 16 - 88.90.63 - 3.50
    Square (mmin) 19x19 - 60x60
    Rectangular (mmin) 25x15 - 100x40
    Wall thickness (mmin) 1.0 - 2.00.039 - 0.079
    Mill length (mm) 6000
    Compare parameters

    Select one parameter to compare

    Comparison

      Shapes
      Circular (mmin)
      Dimensions
      16 - 88.90.63 - 3.50
      Shapes
      Square (mmin)
      Dimensions
      19x19 - 60x60
      Shapes
      Rectangular (mmin)
      Dimensions
      25x15 - 100x40
      Shapes
      Wall thickness (mmin)
      Dimensions
      1.0 - 2.00.039 - 0.079
      Shapes
      Mill length (mm)
      Dimensions
      6000

      Other shapes, sizes and lengths are available upon request.

      Circular Dimensions

      Hide/Show specific columns Edit
      Select columns to display
        Outer diameter (mmin) 1.0 mm (kg/m) 1.25 mm (kg/m) 1.5 mm (kg/m) 2.0 mm (kg/m)
        160.63 0.370 0.455 0.536
        180.71 0.419 0.516 0.610
        190.75 0.444 0.547 0.647 0.838
        200.79 0.469 0.578 0.684 0.888
        220.87 0.518 0.640 0.758 0.986
        250.98 0.592 0.732 0.869 1.13
        281.1 0.666 0.825 0.980 1.28
        301.2 0.715 0.886 1.05 1.38
        321.3 0.765 0.948 1.13 1.48
        351.4 0.838 1.04 1.24 1.63
        381.5 0.912 1.13 1.35 1.78
        401.6 0.962 1.20 1.42 1.87
        411.6 0.990 1.22 1.46 1.92
        44.51.75 1.32 1.58 2.07
        481.9 1.44 1.72 2.27
        502.0 1.50 1.79 2.37
        552.2 1.66 1.98 2.61
        572.2 2.05 2.71
        602.4 2.16 2.86
        763.0 2.76 3.65
        88.93.50 4.29
        Compare parameters

        Select one parameter to compare

        Comparison

          Square Dimensions

          Hide/Show specific columns Edit
          Select columns to display
            Height x Width (mm) 1.0 mm (kg/m) 1.25 mm (kg/m) 1.5 mm (kg/m) 2.0 mm (kg/m)
            19 x 19 0.545 0.665 0.779
            20 x 20 0.576 0.704 0.826
            25 x 25 0.733 0.901 1.06 1.36
            30 x 30 0.890 1.10 1.30 1.68
            32 x 32 0.953 1.18 1.39 1.80
            35 x 35 1.05 1.29 1.53 1.99
            40 x 40 1.77 2.31
            50 x 50 2.24 2.93
            60 x 60 2.71 3.56
            Compare parameters

            Select one parameter to compare

            Comparison

              Rectangular Dimensions

              Hide/Show specific columns Edit
              Select columns to display
                Height x Width (mm) 1.0 mm (kg/m) 1.25 mm (kg/m) 1.5 mm (kg/m) 2.0 mm (kg/m)
                25 x 15 0.576 0.704 0.826
                30 x 10 0.576 0.704 0.826
                30 x 15 0.655 0.802 0.944 1.21
                30 x 20 0.733 0.901 1.06 1.36
                30 x 25 0.785 0.999 1.18 1.52
                35 x 15 0.733 0.901 1.06
                35 x 20 0.812 0.999 1.18 1.52
                40 x 20 0.890 1.10 1.30 1.68
                40 x 25 0.969 1.20 1.42 1.84
                40 x 30 1.05 1.29 1.53 1.99
                50 x 20 1.05 1.29 1.53 1.99
                50 x 25 1.39 1.65 2.15
                50 x 30 1.49 1.77 2.31
                50 x 40 1.69 2.00 2.62
                60 x 20 1.49 1.77 2.31
                60 x 30 1.69 2.00 2.62
                60 x 40 2.24 2.93
                70 x 25 2.12 2.78
                70 x 30 2.24 2.93
                70 x 50 2.71 3.56
                80 x 20 2.24 2.93
                80 x 40 2.71 3.56
                Compare parameters

                Select one parameter to compare

                Comparison

                  Mechanical Properties

                  Hide/Show specific columns Edit
                  Select columns to display
                    Yield strength Rp0.2
                    (min MPa)
                    Tensile strength Rm
                    (min MPa)
                    Elongation A
                    (min %)
                    CR500Y590T-DP 500 590 12
                    CR500Y590T-DH 500 590 20
                    Compare parameters

                    Select one parameter to compare

                    Comparison

                      Chemical Composition (ladle analysis)

                      Hide/Show specific columns Edit
                      Select columns to display
                        C
                        (max %)
                        Si
                        (max %)
                        Mn
                        (max %)
                        P
                        (max %)
                        S
                        (max %)
                        Nb+Ti
                        (max %)
                        Cr+Mo
                        (max %)
                        B
                        (max %)
                        Cu
                        (max %)
                        CR500Y590T-DP 0.15 0.80 2.50 0.050 0.010 0.15 1.40 0.005 0.20
                        CR500Y590T-DH 0.15 0.80 2.50 0.050 0.010 0.15 1.40 0.005 0.20
                        Compare parameters

                        Select one parameter to compare

                        Comparison

                          Chemical composition meets the requirements of VDA 239-100.

                          Tolerances

                          Tolerance Circular

                          Hide/Show specific columns Edit
                          Select columns to display
                            Characteristic Circular precision tubes
                            Tolerances based on the requirements of EN 10305-3
                            Outside diameter (D) (1
                            D < 20 mm
                            20 ≤ D < 32 mm
                            32 ≤ D < 44 mm
                            44 ≤ D < 55 mm
                            55 ≤ D < 70 mm
                            70 ≤ D < 80 mm
                            80 ≤ D < 100 mm

                            ±0.12 mm
                            ±0.15 mm
                            ±0.20 mm
                            ±0.25 mm
                            ±0.30 mm
                            ±0.35 mm
                            ±0.40 mm
                            Out-of-roundness The diameter tolerances include the out-of-roundness
                            Thickness (T) T ≤ 1.5 mm: ±0.15 mm
                            T>1.5 mm: ±10% of nominal thickness or ±0.35 mm whichever is the smaller
                            Straightness Maximum 0.15% of measured length
                            Height of internal weld bead, g;
                            Bead removed
                            Bead not removed

                            g ≤ 0.3 mm
                            g < 0.8 mm, when T ≤ 1.5 mm
                            g < 0.6 x T, when 1.5 mm < T ≤ 3.0 mm
                            Mill length 0/+50 mm, standard length 6000 mm
                            Exact length, single cutting Agreed at the time of enquiry and order
                            Exact length, bundle cutting Agreed at the time of enquiry and order
                            Compare parameters

                            Select one parameter to compare

                            Comparison

                              Characteristic
                              Outside diameter (D) (1
                              D < 20 mm
                              20 ≤ D < 32 mm
                              32 ≤ D < 44 mm
                              44 ≤ D < 55 mm
                              55 ≤ D < 70 mm
                              70 ≤ D < 80 mm
                              80 ≤ D < 100 mm
                              Circular precision tubes
                              Tolerances based on the requirements of EN 10305-3

                              ±0.12 mm
                              ±0.15 mm
                              ±0.20 mm
                              ±0.25 mm
                              ±0.30 mm
                              ±0.35 mm
                              ±0.40 mm
                              Characteristic
                              Out-of-roundness
                              Circular precision tubes
                              Tolerances based on the requirements of EN 10305-3
                              The diameter tolerances include the out-of-roundness
                              Characteristic
                              Thickness (T)
                              Circular precision tubes
                              Tolerances based on the requirements of EN 10305-3
                              T ≤ 1.5 mm: ±0.15 mm
                              T>1.5 mm: ±10% of nominal thickness or ±0.35 mm whichever is the smaller
                              Characteristic
                              Straightness
                              Circular precision tubes
                              Tolerances based on the requirements of EN 10305-3
                              Maximum 0.15% of measured length
                              Characteristic
                              Height of internal weld bead, g;
                              Bead removed
                              Bead not removed
                              Circular precision tubes
                              Tolerances based on the requirements of EN 10305-3

                              g ≤ 0.3 mm
                              g < 0.8 mm, when T ≤ 1.5 mm
                              g < 0.6 x T, when 1.5 mm < T ≤ 3.0 mm
                              Characteristic
                              Mill length
                              Circular precision tubes
                              Tolerances based on the requirements of EN 10305-3
                              0/+50 mm, standard length 6000 mm
                              Characteristic
                              Exact length, single cutting
                              Circular precision tubes
                              Tolerances based on the requirements of EN 10305-3
                              Agreed at the time of enquiry and order
                              Characteristic
                              Exact length, bundle cutting
                              Circular precision tubes
                              Tolerances based on the requirements of EN 10305-3
                              Agreed at the time of enquiry and order

                              1)For a maximum distance of 100 mm, the ends may, due to the cutting method, have diameters outside the tolerances.

                              Tolerance Square

                              Hide/Show specific columns Edit
                              Select columns to display
                                Characteristic Square precision tubes
                                Tolerances meet or exceed the requirements of EN 10305-5
                                Outside dimensions (H) and (B), longer side1)
                                H < 25 mm
                                25 ≤ H < 40 mm
                                40 ≤ H < 60 mm
                                60≤ H < 70 mm

                                ±0.20 mm
                                ±0.25 mm
                                ±0.30 mm
                                ±0.35 mm
                                Side concavity and convexity Included in outside dimension tolerance
                                Thickness (T) T≤ 1.5 mm: ±0.15 mm
                                T>1.5 mm: ±10% of nominal thickness or ±0.35 mm whichever is the smaller
                                Straightness Maximum 0.15% of measured tube length when shorter side length > 30 mm
                                Maximum 0.25% of measured tube length when the shorter side length ≤ 30 mm
                                Location of weld seam from the centre line On narrow side for square and rectangular, optionally on wide side. On wide side for flat oval and ellipse. ± 10% of side length or ± 3 mm, whichever is greater.
                                Height of internal weld bead, g;
                                Bead removed
                                Bead not removed

                                g ≤ 0.3 mm
                                g < 0.8 mm, when T ≤ 1.5 mm
                                g < 0.6 x T, when 1.5 mm < T ≤ 3.0 mm
                                Squareness of side 90° ±1°
                                Corner profile R ≤ 3.0 x T, typically R ≤ 2.0 x T
                                Twist (V) V ≤ 3 mm for B and H ≤ 30 mm
                                V ≤ B/10 or ≤ H/10 for B or H > 30 mm
                                Mill length 0/+50 mm, standard length 6000 mm
                                Exact length, single cutting Agreed at the time of enquiry and order
                                Exact length, bundle cutting Agreed at the time of enquiry and order
                                Compare parameters

                                Select one parameter to compare

                                Comparison

                                  Characteristic
                                  Outside dimensions (H) and (B), longer side1)
                                  H < 25 mm
                                  25 ≤ H < 40 mm
                                  40 ≤ H < 60 mm
                                  60≤ H < 70 mm
                                  Square precision tubes
                                  Tolerances meet or exceed the requirements of EN 10305-5

                                  ±0.20 mm
                                  ±0.25 mm
                                  ±0.30 mm
                                  ±0.35 mm
                                  Characteristic
                                  Side concavity and convexity
                                  Square precision tubes
                                  Tolerances meet or exceed the requirements of EN 10305-5
                                  Included in outside dimension tolerance
                                  Characteristic
                                  Thickness (T)
                                  Square precision tubes
                                  Tolerances meet or exceed the requirements of EN 10305-5
                                  T≤ 1.5 mm: ±0.15 mm
                                  T>1.5 mm: ±10% of nominal thickness or ±0.35 mm whichever is the smaller
                                  Characteristic
                                  Straightness
                                  Square precision tubes
                                  Tolerances meet or exceed the requirements of EN 10305-5
                                  Maximum 0.15% of measured tube length when shorter side length > 30 mm
                                  Maximum 0.25% of measured tube length when the shorter side length ≤ 30 mm
                                  Characteristic
                                  Location of weld seam from the centre line
                                  Square precision tubes
                                  Tolerances meet or exceed the requirements of EN 10305-5
                                  On narrow side for square and rectangular, optionally on wide side. On wide side for flat oval and ellipse. ± 10% of side length or ± 3 mm, whichever is greater.
                                  Characteristic
                                  Height of internal weld bead, g;
                                  Bead removed
                                  Bead not removed
                                  Square precision tubes
                                  Tolerances meet or exceed the requirements of EN 10305-5

                                  g ≤ 0.3 mm
                                  g < 0.8 mm, when T ≤ 1.5 mm
                                  g < 0.6 x T, when 1.5 mm < T ≤ 3.0 mm
                                  Characteristic
                                  Squareness of side
                                  Square precision tubes
                                  Tolerances meet or exceed the requirements of EN 10305-5
                                  90° ±1°
                                  Characteristic
                                  Corner profile
                                  Square precision tubes
                                  Tolerances meet or exceed the requirements of EN 10305-5