SSAB Form 200 Hot-Rolled

Download data sheet

General Product Description

SSAB Form 200 is a mild steel intended for forming with the best conceivable properties in both drawing and stretch forming operations. SSAB Form 200 is used for a wide variety of applications including vehicle parts, refrigerators, electric radiators and water radiators.

Dimension Range

SSAB Form 200 is available in thicknesses of 1.80-15.00 mm and widths up to 1860 mm as coils, slit coils and as cut to length in lengths up to 16 meters.

Mechanical Properties

Thickness
(mmin)
Thickness
(mmin)
1.80 - 3.000.0709 - 0.118
Yield strength ReH
(max MPa)
300
Tensile strength Rm
(max MPa)
400
Elongation A80
(min %)
33
Elongation A5 1)
(min %)
37
Min. inner bending radius for a 90° bend
(x t)
0.0
Thickness
(mmin)
Thickness
(mmin)
3.01 - 6.000.119 - 0.236
Yield strength ReH
(max MPa)
300
Tensile strength Rm
(max MPa)
400
Elongation A80
(min %)
—
Elongation A5 1)
(min %)
37
Min. inner bending radius for a 90° bend
(x t)
0.0
Thickness
(mmin)
Thickness
(mmin)
6.01 - 15.000.237 - 0.5906
Yield strength ReH
(max MPa)
300
Tensile strength Rm
(max MPa)
400
Elongation A80
(min %)
—
Elongation A5 1)
(min %)
37
Min. inner bending radius for a 90° bend
(x t)
0.4

The mechanical properties are tested in the transverse direction.

1) A5 value applies for thicknesses ≥ 3.00 mm.

Chemical Composition (heat analysis)

C
(max %)
C
(max %)
0.065
Si
(max %)
0.03
Mn
(max %)
0.35
P
(max %)
0.030
S
(max %)
0.025
Al
(min %)
0.015

The steel is grain refined.

Tolerances

SSAB Form is delivered with SSAB Form tolerances, with improved guarantees compared to EN 10051. More details are available at SSAB.com

Thickness

SSAB Form thickness tolerances correspond to EN 10051 tolerances for deep drawing steels according to EN 10111 as default value. After special agreement tighter tolerances can be delivered for certain products and dimensions.

Length and Width

SSAB Form tolerances for width and length are according to SSAB standard. The SSAB standard offer narrower width and length tolerances compared to EN 10051.

For coil and sheet with mill edge, the width tolerances are corresponding to -0/+20 mm.

For coil and sheet with cut edge, the width tolerances are corresponding to -0/+2 mm.

After special agreement, tighter tolerances can be delivered for certain products and dimensions.

Length tolerances only apply for cut to length sheets.

Shape

Tolerances according to EN 10051.

Flatness

SSAB Form tolerances guarantee a maximum flatness deviation of 3 mm/m in addition to the EN 10051 flatness requirements.

Flatness guarantees only apply for cut to length sheets.

Surface Properties

According to EN 10163-2 Class A, Subclass 3.

Delivery Conditions

Thermomechanically rolled.

Surface and edge condition

SSAB Form 200 is available with non-pickled or pickled surface with mill or cut edge.

Fabrication and Other Recommendations

SSAB Form 200 has good cold forming, welding and cutting performance especially laser-cutting.

SSAB Form 200 is suitable for hot dip galvanizing.

For information concerning fabrication, see SSAB´s brochures on www.ssab.com or consult Tech Support.

Appropriate health and safety precautions must be taken when bending, welding, cutting, grinding or otherwise working on the products.

Contact Information

www.ssab.com/contact 
Copyright 2026