    Laminate FoodSafe from SSAB is available in white colors with a low gloss smooth surface, but can also be supplied with enhanced antistatic properties to minimize the contamination from airborne particles like dust. 

    Laminate FoodSafe has typically a metal coated steel substrate with primer, adhesive and PVC-laminate on top side. Each layer is optimized for performance and processing benefits. 

    Laminate FoodSafe offers excellent formability for a wide range of applications including walls, ceilings, doors in cold rooms and deep freezers, as well as refrigerated counters, institutional kitchens and production premises. 

    Laminate FoodSafe is a highly durable and wear resistant laminated steel product that is resistant to chemicals and detergents which makes it easy to clean. It is non-toxic and suitable for direct contact with food and fully complies with current EU regulations (EU) No 10/2011, REACH regulations and is fully free of chromates.

    The reverse side of the sheet is painted with a two-layer grey backside coating.

    SSAB’s color coated steels are all manufactured according to EN 10169.
     

    Technical Properties

    Hide/Show specific columns Edit
    Select columns to display
      Technical Properties
      Gloss 11
      Minimum inner bending radius 1 x sheet thickness
      Scratch resistance 55 N
      Highest operating temperature 60 °C
      Lowest operating temperature -40 °C
      Coating thickness, nominal (primer + top coat) 120 µm
      Primer thickness, nominal 6 µm
      Coating structure Smooth
      Steel designation 1) S250GD-S350GD, DX51D
      Zinc coating 275 g/m2
      Min steel thickness 1) 0.42 mm
      Steel width 1) 1000 - 1400 mm
      Compare parameters

      Select one parameter to compare

      Comparison

        Technical Properties
        Gloss
        11
        Technical Properties
        Minimum inner bending radius
        1 x sheet thickness
        Technical Properties
        Scratch resistance
        55 N
        Technical Properties
        Highest operating temperature
        60 °C
        Technical Properties
        Lowest operating temperature
        -40 °C
        Technical Properties
        Coating thickness, nominal (primer + top coat)
        120 µm
        Technical Properties
        Primer thickness, nominal
        6 µm
        Technical Properties
        Coating structure
        Smooth
        Technical Properties
        Steel designation 1)
        S250GD-S350GD, DX51D
        Technical Properties
        Zinc coating
        275 g/m2
        Technical Properties
        Min steel thickness 1)
        0.42 mm
        Technical Properties
        Steel width 1)
        1000 - 1400 mm

        1) Maximum steel thickness is 1.5 mm and maximum steel width depends on steel thickness. For other steel dimensions or steel grades please contact SSAB Tech Support.

        Colors

        Laminate FoodSafe is available in white colors.

        Reverse Side Coating

        Unless otherwise specified, the reverse side of the sheet is painted with a two-layer coating to further improve the corrosion resistance of the end product. The coating provides good adhesion properties to many adhesives and foams; nevertheless the compatibility needs to be tested case-specifically.

        Hide/Show specific columns Edit
        Select columns to display
          Technical Properties
          Nominal Coating Thickness (primer + top coat) 12 µm
          Color Grey
          Corrosion Resistance Min CPI3
          Compare parameters

          Select one parameter to compare

          Comparison

            Technical Properties
            Nominal Coating Thickness (primer + top coat)
            12 µm
            Technical Properties
            Color
            Grey
            Technical Properties
            Corrosion Resistance
            Min CPI3

            For easy material identification the reverse side of the sheet is stamped with the SSAB logo and the product name. The production year is marked to ease material traceability and can be referred to within the guarantee period. An arrow shows the direction of production to ensure installation in a uniform direction.

            Contact Information

            www.ssab.com/contact