Martensitic steel: excellent formability-to-strength ratio

Martensitic steel combines tensile strengths up to 1700 MPa with good ductility, making it highly efficient for both vehicle lightweighting and improved crash protection — especially in anti-intrusion zones.

What is the definition of martensitic steel?

When austenite iron is very rapidly quenched, the austenite is transformed into a very hard crystalline microstructure called “martensite.”

The martensitic transformation begins when the austenite reaches the martensite start temperature (Ms) and continues until the lower transformation temperature (Mt) is reached. In general, the higher the percentage of conversion to martensite, the stronger the resulting martensitic steel. These steels undergo post-quench martensitic tempering to improve their ductility, so that even MS steels with very high strength levels can be cold-formed using processes like cold-roll forming.

To produce cold-rolled martensitic steel (aka MS or MART), a cold-rolled steel strip is fed into a continuous annealing line (CAL). In the CAL, the material is annealed, water-quenched, and tempered. The austenite formed in the CAL, when rapidly quenched, is transformed into martensite. The CAL’s tempering operation provides the ultra-high strength steel with improved ductility.

Docol® martensitic grades have less than 2% alloying elements, providing good weldability.

Martensitic steel properties

  • Extremely high yield strength (Rp0,2) and tensile strength (Rm).
  • Superior energy absorption and impact strength for anti-intrusion zones.
  • Ideal for vehicle lightweighting.
  • Cold formability in bending, stamping, and roll-forming — including 3D forming.
  • Martensitic steel is significantly more cost-effective than aluminum: using optimized design profiles, MS steels can deliver high-strength performance that is similar to aluminum and at the same weight.

Where are martensitic steels used on cars?

With the highest strength of our cold-formable steels, Docol martensitic steel enables excellent lightweighting and increased crash performance:

  • EV battery protection
  • Sill (rocker) reinforcements
  • Door/side intrusion beams
  • Bumpers
  • Roof reinforcements
  • Seat structures

 

Martensitic steel for automotive applications

Our strongest martensitic steel – now in use

DOCOL 1700M

Cold-rolled Docol 1700M steel from SSAB is an eco-friendly, pound-for-pound alternative to aluminum for lightweight components used in passive safety systems. Due to Docol martensitic steel’s ductility, critical safety components are now being fabricated using cost- and energy-efficient cold forming processes.

For example, Shape Corp. uses 3D roll-forming to create lighter, more compact, and stronger A-pillars and roof rail tubes in Docol martensitic 1700MPa. Designed for the Ford 2020 Explorer and 2020 Escape, these key safety components increase driver visibility, interior space, and air bag placement optimization.

Docol 1700 martensitic is the material of choice for ultra-high strength steel (UHSS) applications, including side impact beams, bumpers, structural components, and EV battery enclosures. Docol design specialists can provide stimulated crash performance data on several optimized 1700MPa profiles, as well as simulations for many of our other martensitic grades: Docol 900M, 1100M, 1200M, 1300M, 1400M and 1500M.

Grades and mechanical properties for Docol martensitic steel

For best weight reduction, use higher grades with reduced thicknesses. Corrosion-resistant martensitic grades: electrogalvanized (EG) coatings are available on Docol 900M, Docol 1100M, Docol 1200M, Docol 1300M, Docol 1400M, and Docol 1500M. All Docol martensitic steel grades are available cold rolled (CR); Docol 1200M is available both cold rolled and hot rolled (HR). For more details, please download the data sheets listed below.
Product Family

Docol 900M

Product name
Docol CR​700Y​900T-​MS
Coating
UC, EG
Dimensions
T: 0.50 - 2.10 mm
W: Up to 1527 mm
T: 0.020 - 0.0827 in
W: Up to 60.12 in
Standards
SSAB
Datasheet
Product Family

Docol 1100M

Product name
Docol CR​860Y​1100T-​MS
Coating
UC, EG
Dimensions
T: 0.50 - 2.00 mm
W: Up to 1527 mm
T: 0.020 - 0.0787 in
W: Up to 60.12 in
Standards
SSAB
Datasheet
Product Family

Docol 1200M

Product Family

Docol 1300M

Product name
Docol CR​1030Y​1300T-​MS
Coating
UC, EG
Dimensions
T: 0.50 - 2.10 mm
W: Up to 1527 mm
T: 0.020 - 0.0827 in
W: Up to 60.12 in
Standards
VDA 239-100
Datasheet
Product Family

Docol 1400M

Product name
Docol CR​1150Y​1400T-​MS
Coating
UC, EG
Dimensions
T: 0.50 - 2.10 mm
W: Up to 1527 mm
T: 0.020 - 0.0827 in
W: Up to 60.12 in
Standards
SSAB
Datasheet
Product Family

Docol 1700M

Product name
Docol CR​1350Y​1700T-​MS
Coating
UC
Dimensions
T: 1.00 - 2.10 mm
W: Up to 1250 mm
T: 0.0394 - 0.0827 in
W: Up to 49.21 in
Standards
VDA 239-100
Datasheet

*Available upon request.

Forming Docol martensitic steel

  • Excellent cold formability for bending, roll-forming, and stamping at room temperatures.
  • Quite good drawability and good edge-stretching and hole-expansion properties.
  • Good weldability, including resistance spot welding and laser welding.
  • Docol® martensitic steel grades are highly consistent — in their mechanical properties — avoiding stresses that can lead to unwanted or unexpected springback.
For specific forming guidance for your martensitic steel automotive component, please contact our Technical Support.
Martensitic steel has excellent cold formability

Additional benefits from Docol martensitic steel

  • Superior fatigue properties for all vehicles: BEV, ICE or hybrid.
  • Seven high-strength grades: 900MPa, 1100MPa, 1200MPa, 1300MPa, 1400MPa, 1500MPa and 1700MPa.
  • Grades are available to meet OEM-specific standards and certifications.
  • Electrogalvanized (EG) corrosion resistance available on request.
  • Global availability and support. All grades listed are now commercially available.

Are you looking for OEM specific grades?

Docol® steel grades can be supplied according to OEM or VDA standards. And, in close cooperation with automotive OEMs, we often develop innovative AHSS steels that are customized for a specific car application. If we don’t list a specific grade that you need, contact our technical support for more information.

Custom AHSS for automotive OEMs

The benefits of Docol® martensitic steel for each team member

Safety engineers: Create new anti-intrusion zones (e.g., for BEV battery packs) and optimize the space utilization of existing zones (e.g., passenger compartments).

Lightweighting engineers: Leverage the extreme steel strength and aluminum-like weight of martensitic steel.

Production engineers: Use familiar cold forming operations (bending, stamping, roll-forming) and exciting new operations, like 3D roll-forming, on a UHSS steel.

Procurement officers: Realize major cost reductions — with no performance penalty — by replacing aluminum with Docol martensitic steel. (And reduce your carbon footprint at the same time.)

Sustainability officers: Lower the embedded CO2 in your materials and improve your life cycle assessment with our “future-proofed” Docol martensitic steels.


Future-proof your life cycle assessment
Lower your embedded CO2

Docol martensitic steel is "future-proofed".

Electrogalvanized martensitic steel

Docol electrogalvanized MS steels provide corrosion resistance using a uniform, high quality, protective coating, which can be applied as a very thin coat, if desired. Docol EG-coated martensitic grades can be readily formed and joined, with excellent resistance spot welding (RSW) properties.

Docol EZ (or ZE) martensitic automotive steels are available from SSAB in the following strengths: Docol 900M, 1100M, 1200M, 1300M, 1400M and 1500M. With SSAB’s long and extensive experience in making electrogalvanized martensitic steels, car OEMs can have any of their concerns regarding hydrogen embrittlement (HE), also known as hydrogen-induced cracking (HIC), fully addressed.

High yield strength martensite for crash performance

World Auto Steel points out a correlation between sheet steel yield strength and the 3-point bending deformation (crash behavior) of hat-shaped parts:
“CR1200Y1470T-MS has similar performance to hot-stamped PHS-CR1800T-MB and PHS-CR1900T-MB at the same thickness, and exceeds the frequently used PHS-CR1500T-MB. For this reason, there may be the potential to reduce costs and even weight with a cold-stamping approach, providing appropriate press, process, and die designs are used.” World Auto Steel’s Metallurgy of Martensitic Steels.

coils
TRIAL MATERIAL STOCK

Try it for yourself

With our Trial Material Stock Center, you can get AHSS samples for most of our commercially available steels – as well as samples for our newest but not yet commercially released grades. Unique to the industry, we ship coils, sheets and custom lengths of any size. In 1 to 2 weeks, your material is ready for dispatch to anywhere in the world.

FAQ

Dual phase with high formability

Dual phase with high formability/ductility for crack-free cold deep drawing

Dual phase with high formability/ductility (DH) steels are TRIP-assisted, 3rd Generation automotive steels with high global and local formability and good resistance to edge cracking. DH steel have excellent energy-absorbing properties, included reserved ductility during crash impact. DH grades are ideal for complex geometries, including cold deep drawing. DH steel's FLDs and HERs are superior to DP steels, enabling scrap reduction and more streamlined stamping.

Read more
press hardening steel

Press hardening steels (PHS) for complex shapes

Press hardening steels have four major advantages: they can be formed into very complex shapes, their ultimate tensile strength ranges up to 2000 MPa (290 ksi), there is little or no springback, and, with tailored tempering, you can combine “full hard zones” and “soft zones” for multi-function crash performance within a single part.

Read more
Docol complex phase steel

Complex phase (CP) steels for the highest hole expansion ratios

Complex phase steels have the highest — up to 75% — hole expansion ratios available from advanced high strength steels. Their high HER values provide excellent cold-forming properties for punched and stretched edges/flanges, as well as deep-drawn shapes. CP steels’ superior yield strengths are used for high crash-energy absorption, while their elevated UTS levels enable thinner walls for significant automobile weight reductions.

Read more

Dual phase (DP) steel: excellent ductility and energy absorption

Dual phase automotive steels have an excellent balance of ductility, high tensile strengths, easy cold formability, and very good crash energy-absorption. Its high early-stage strain hardening (n-value) makes DP steel resistant to local necking due to strain redistribution — providing highly uniform elongation. Dual phase steel’s low yield-to-tensile-strength ratio creates high global formability for deep-drawing and high-stretching capacities — all with good weldability.

Read more
Docol High Edge ductility

High edge (HE) ductility HSLA steel

High edge ductility HSLA steel with greatly improved local formability and high hole expansion ratios – ideal for challenging auto components with complex designs on sheared stretched edges.

Read more

High strength, low alloy (HSLA) steels for cost-effective automotive lightweighting

High strength, low alloy steels are a cost-effective choice for increasing strength-to-weight ratios when compared to conventional mild carbon steels. HSLA steels also have excellent bendability and weldability and can increase the strength and/or decrease the weight for a variety of body-in-white and chassis automotive components, including suspensions, beams, and subframes.

Read more

Ferritic-Bainitic steel: stretch edge flangeability for cold-forming

Ferritic-Bainitic are multi-phased steels with high hole expansion ratios and good edge stretch capabilities. FB steels are suited for cold-formed and punched flanges when lightweighting automotive components such as wheels, cross members, and other structural parts.

Read more