Armox® 440T

Download data sheet

General Product Description

Blast protection plate.

Armox® 440T combines excellent penetration and shock resistance. It offers vehicle designers new ways to increase protection using lighter weight designs.

Benefits of using Armox® 440T include: 

 

  • Superior workshop properties
  • Optimized solutions
  • Perfect hardness/toughness balance, for combined penetration and blast protection
  • Expertise in ballistic protection from SSAB

 

Armox® 440T is not intended for further heat treatment.

 

Mechanical Properties

Thickness
(mmin)
Thickness
(mmin)
4.0 - 30.00.157 - 1.1810
Hardness
(HBW)
420 - 480
Yield strength Rp0.2
(min MPaksi)
1100159
Tensile strength Rm
(MPaksi)
1250 - 1550181 - 224
Elongation A5
(min %)
10
Thickness
(mmin)
Thickness
(mmin)
30.1 - 50.01.185 - 1.968
Hardness
(HBW)
420 - 480
Yield strength Rp0.2
(min MPaksi)
1050152
Tensile strength Rm
(MPaksi)
1250 - 1550181 - 224
Elongation A5
(min %)
10
Thickness
(mmin)
Thickness
(mmin)
50.1 - 80.01.972 - 3.150
Hardness
(HBW)
420 - 480
Yield strength Rp0.2
(min MPaksi)
1000145
Tensile strength Rm
(MPaksi)
1250 - 1550181 - 224
Elongation A5
(min %)
10

Mechanical Testing

Brinell hardness test according to EN ISO 6506-1 on each heat treatment individual.

Charpy impact test according to EN ISO 148 on each heat and thickness from 6 mm.

Tensile test according to EN ISO 6892 on each heat and thickness. 

 

Ultrasonic testing

According to EN 10160 Class E3S3.

 

Impact Properties

Thickness
(mmin)
Thickness
(mmin)
4.0 - 80.00.157 - 3.150
Min impact energy for transversal testing,
Charpy V 10x10 mm test specimen 1)
45 J / -40 °C33 ft-lbs / -40 °F

1) Average of three tests. Transverse to rolling direction. Single value min. 70% of specified average. For plate thicknesses under 12 mm sub-size Charpy-V specimen are used. The specified minimum value is then propotional to the specimen cross-section.

 

 

Chemical Composition (ladle analysis)

C *)
(max %)
C *)
(max %)
0.21
Si *)
(max %)
0.50
Mn*)
(max %)
1.20
P
(max %)
0.010
S
(max %)
0.003
Cr*)
(max %)
1.0
Ni*)
(max %)
2.50
Mo*)
(max %)
0.70
B*)
(max %)
0.005

Tolerances

More details are given in SSAB brochure Armox® Guarantees or on www.ssab.com.

Thickness

Tolerances according to Armox® Thickness Guarantees.

Armox® Guarantees meet the requirements of EN 10029 Class C, but offers narrower tolerances.

Length and Width

Tolerances conform to EN 10029 or to SSAB´s standard after agreement.

Dimensional tolerances for plate with mill edge according to special agreement. 

Shape

Tolerances according to EN 10029.

Flatness

Tolerances according to Armox® flatness guarantees, which are more restrictive than EN 10029 Class N (steel type L).

Surface Properties

According to EN 10163-2 Class B, Subclass 3.

Delivery Conditions

The delivery condition is QT (Quenched and Tempered).

 

Delivery requirements can be found in SSAB’s brochure Armox® Guarantees or www.ssab.com.