General Product Description

Strenx® 1100 E/F is a structural steel with a high yield strength at a minimum of 1100 MPa.

Typical applications include demanding load-bearing structures. Despite its strength, the material is surprisingly easy to weld and bend.

Benefits include:

  • Superior bendability and surface quality
  • Weldability with excellent HAZ strength and toughness
  • Exceptional consistency within a plate guaranteed by close tolerances
  • High impact toughness which provides for good resistance to fractures

Dimension Range

 Strenx® 1100 E/F is available in plate thicknesses of 4.0 – 40.0 mm. Strenx® 1100 is available in widths up to 3200 mm and lengths up to 14630 mm depending on thickness. More detailed information on dimensions is provided in the dimension program.

Mechanical Properties

Hide/Show specific columns Edit
Select columns to display
    Thickness
    (mmin)
    Yield strength Rp0.2
    (min MPaksi)
    Tensile strength Rm
    (MPaksi)
    Elongation A5
    (min %)
    4.0 - 4.90.157 - 0.193 1100160 1250 - 1550181 - 224 8
    5.0 - 40.00.197 - 1.575 1100160 1250 - 1550181 - 224 10
    Compare parameters

    Select one parameter to compare

    Comparison

      For transverse test pieces.

      Impact Properties

      Hide/Show specific columns Edit
      Select columns to display
        Product Min impact energy for transversal testing,
        Charpy V 10x10 mm test specimen 1)
        Strenx® 1100 E 27 J / -40 °C20 ft-lbs / -40 °F
        Strenx® 1100 F 27 J / -60 °C20 ft-lbs / -76 °F
        Compare parameters

        Select one parameter to compare

        Comparison

          Product
          Strenx® 1100 E
          Min impact energy for transversal testing,
          Charpy V 10x10 mm test specimen 1)
          27 J / -40 °C20 ft-lbs / -40 °F
          Product
          Strenx® 1100 F
          Min impact energy for transversal testing,
          Charpy V 10x10 mm test specimen 1)
          27 J / -60 °C20 ft-lbs / -76 °F

          1) Unless otherwise agreed, transverse impact testing according to EN 10025-6 option 30 will apply. For thicknesses between 6 - 11.9 mm, sub-size Charpy V-specimens are used. The specified minimum value is then proportrional to the cross-sectional area of the specimen compared to a full-size specimen (10 x 10 mm).

          Chemical Composition (ladle analysis)

          Hide/Show specific columns Edit
          Select columns to display
            C *)
            (max %)
            Si *)
            (max %)
            Mn*)
            (max %)
            P
            (max %)
            S
            (max %)
            Cr*)
            (max %)
            Cu*)
            (max %)
            Ni*)
            (max %)
            Mo*)
            (max %)
            B*)
            (max %)
            0.21 0.50 1.40 0.020 0.005 0.80 0.30 3.0 0.70 0.005
            Compare parameters

            Select one parameter to compare

            Comparison

              The steel is grain refined. *) Intentional alloying elements.

              Carbon Equivalent CET(CEV)

              Hide/Show specific columns Edit
              Select columns to display
                Thickness (mmin) 4.0 - 4.90.157 - 0.193 5.0 - 8.00.197 - 0.315 8.1 - 15.00.319 - 0.591 15.1 - 40.00.594 - 1.575
                Strenx® 1100 E Max CET(CEV) 0.37 (0.57) 0.38 (0.58) 0.39 (0.62) 0.42 (0.73)
                Strenx® 1100 F Max CET(CEV) 0.40 (0.70) 0.40 (0.70) 0.42 (0.73)
                Compare parameters

                Select one parameter to compare

                Comparison

                  CET and CEV formula

                  Tolerances

                  More details are given in SSAB’s brochure Strenx® Guarantees.

                  Thickness

                  Tolerances according to Strenx® Thickness Guarantees.

                  Strenx® Guarantees meet the requirements of EN 10029 Class A, but offers narrower tolerances.

                  Length and Width

                  According to SSAB’s dimension program. Tolerances conforms with EN 10 029. 

                  Shape

                  Tolerances according to EN 10029.

                  Flatness

                  Tolerances according to Strenx® Flatness Guarantee Class D, which are more narrow than EN 10029 Class N.

                  Surface Properties

                  According to EN 10163-2 Class A, Subclass 3.

                  Delivery Conditions

                  The delivery condition is Quenched and Tempered. The plates are delivered with sheared or thermally cut edges. Untrimmed edges after agreement.

                  Delivery requirements can be found in SSAB’s brochure Strenx® Guarantees or on www.ssab.com.

                  Fabrication and Other Recommendations

                  Welding, bending and machining

                  Recommendations are found in SSAB’s brochures at www.ssab.com or consult Tech Support.

                  Strenx® 1100 E/F has bending guarantees according to Strenx® Bending Guarantees Class C.

                  Strenx® 1100 E/F has obtained its mechanical properties by quenching and subsequent tempering. The properties of the delivery condition cannot be retained after exposure to temperatures in excess of 200ºC.

                  Appropriate health and safety precautions must be taken when welding, cutting, grinding or otherwise working on this product. Grinding, especially of primer coated plates, may produce dust with a high particle concentration.