Normalized pressure vessel steel heavy plate dual certified to structural steel.

SSAB Multisteel PES is hot rolled structural steel for general pressure equipment steel constructions. PES = Pressure European Structural (meets the European standard).

Exceeding the requirements of several standard steel grades, SSAB Multisteel PES is a versatile pressure vessel steel for fabricated pressure equipment made of weldable fine grain steels. Formability and highly consistent quality guarantee fast, uninterrupted production, generating clear savings in the costs of material management. Certification also to structural steel according to EN 10025-2 gives more possibilities to use in several applications.

SSAB Multisteel PES exceeds several steel standards and is available as four steel grades: SSAB Multisteel PES, P355N, P355NH and P355NL2 according to EN 10028-3 and furthermore S355K2+N according to EN 10025-2.

SSAB Multisteel PES covers steel grades in four different qualities:

1) Room temperature quality (P355N)

2) Elevated temperature quality (P355NH)

3) Special low temperature quality (P355NL2)

4) Structural quality (S355K2+N)

5) SSAB Multisteel PES (all together)

PED certificate:

Pressure vessel steel grades recognized by standard EN 10028 are mainly delivered with the inspection certificate 3.1. Directive 2014/68/EU (PED) requires the manufacturer’s quality assurance system to be approved by an external accredited authority (Notified Body).

SSAB Europe Oy Raahe Works holds the PED – approval from DNV.

SSAB Raahe Works is authorized to use PED certificate for pressure equipment steels according to EN 10028-3 based on EN 10028-1.

Dimension Range

SSAB Multisteel PES is available in thickness of 5.00 – 150.00 mm.

Mechanical Properties

Hide/Show specific columns Edit
Select columns to display
    Thickness
    (mmin)
    Yield strength
    (min MPa)
    Tensile strength
    (MPa)
    Elongation A5
    (min %)
    5.00 - 16.000.197 - 0.6299 355 490 - 630 22
    16.01 - 40.000.6303 - 1.575 345 490 - 630 22
    40.01 - 60.001.575 - 2.362 335 490 - 630 22
    60.01 - 63.002.363 - 2.480 335 470 - 610 21
    63.01 - 80.002.481 - 3.150 325 470 - 610 21
    80.01 - 100.003.150 - 3.9370 315 470 - 610 21
    100.01 - 150.003.9374 - 5.9055 305 460 - 600 21
    Compare parameters

    Select one parameter to compare

    Comparison

      The mechanical properties are tested transverse to the direction of rolling.

      Hot tensile test is performed at +300°C in compliance with EN 10028-3 and EN 10028-1.

      Impact Properties

      Hide/Show specific columns Edit
      Select columns to display
        Min. impact energy for longitudinal testing,
        Charpy V 10x10 mm test specimens
        SSAB Multisteel PES 27 J / -50 °C
        EN 10028-3 P355N, P355NH 30 J / -20 °C
        EN 10028-3 P355NL2 27 J / -50 °C
        EN 10028-3 S355K2+N 40 J / -20 °C
        Compare parameters

        Select one parameter to compare

        Comparison

          SSAB Multisteel PES
          Min. impact energy for longitudinal testing,
          Charpy V 10x10 mm test specimens
          27 J / -50 °C
          EN 10028-3 P355N, P355NH
          Min. impact energy for longitudinal testing,
          Charpy V 10x10 mm test specimens
          30 J / -20 °C
          EN 10028-3 P355NL2
          Min. impact energy for longitudinal testing,
          Charpy V 10x10 mm test specimens
          27 J / -50 °C
          EN 10028-3 S355K2+N
          Min. impact energy for longitudinal testing,
          Charpy V 10x10 mm test specimens
          40 J / -20 °C

          The impact test is made transverse to the rolling direction in compliance with EN 10028-3 and EN 10028-1 (EN 10025-2 and EN 10025-1).

          Chemical Composition (ladle analysis)

          Hide/Show specific columns Edit
          Select columns to display
            C
            (max %)
            Si
            (max %)
            Mn
            (max %)
            P
            (max %)
            S
            (max %)
            Nb
            (max %)
            0.18 0.50 1.60 0.020 0.005 0.05
            Compare parameters

            Select one parameter to compare

            Comparison

              Carbon Equivalent CEV

              Hide/Show specific columns Edit
              Select columns to display
                Thickness (mmin) 5.00 - 50.000.197 - 1.969 50.01 - 150.001.969 - 5.9055
                CEV (max %) 0.43 0.45
                Compare parameters

                Select one parameter to compare

                Comparison

                  Tolerances

                  Thickness ¾ from EN 10029 Class B.

                  Width and length according to EN 10029.

                  Flatness tolerance 6 mm/m.

                  Surface according to EN 10163-2 Class B subclass 3.

                  Delivery Conditions

                  Normalized.

                  Coating

                  Shot blasted & primed surface is available upon request.

                  Certificates

                  SSAB Multisteel PES provides three different certificates:

                  EN 10204-3.1 to SSAB Multisteel PES.

                  EN 10204-3.1/PED2014/68/EU to P355NL2/NH/N EN 10028-3.

                  EN 10204-3.1 +CE to S355K2+N EN 10025-2.

                  Fabrication and Other Recommendations

                  Welding:

                  Weldability is excellent with all welding processes. Increased working temperature requirements are less than those of the corresponding strength grades of standard steels. This means easier welding and cost savings under both workshop and site welding conditions.

                  Needed working temperatures for thick plates please consult SSAB Tech Support.

                  Forming:

                  SSAB Multisteel offers better formability properties than standard steels. Successful forming requires that the manufacturer uses good workshop techniques. Worn tools, poor lubrication, scratches on the surface of the steel as well as edge burrs will all reduce forming quality.

                  Guaranteed minimum bending radius for all directions is 2 x t up to 30 mm thick plate where t = plate thickness.

                  Heat treatment:

                  Recommendations for stress relieving and normalizing.

                  Stress relieving 550 – 600°C (target 580°C)

                  2 minutes/millimeter of thickness, however, 30 minutes minimum. Slow cooling in the furnace.

                  Normalizing 900 – 940°C (target 920°C)

                  1 minute/millimeter of thickness, however, 20 minutes minimum. Cooling in free air.

                  For information concerning fabrication, see SSAB´s brochures on www.ssab.com or consult Tech Support.

                  Appropriate health and safety precautions must be taken when bending, welding, cutting, grinding or otherwise working on the products.

                  Contact Information

                  www.ssab.com/contact