Docol® S650MC high strength low alloy

Download data sheet

General Product Description

The high-strength structural steel Docol S650MC is a hot-rolled steel made for cold forming, with a minimum yield strength of 650 MPa for stronger and lighter structures. Docol S650MC meets or exceeds the requirements of S650MC in EN 10149-2. Typical applications include a wide range of heavy trucks components and parts, such as frame rails and cross-members. Docol S650MC comes in coils, slit coils and cut-to-length sheets.

Dimension Range

Hot rolled / UC: thickness 2.00-10.00 mm, width up to 1600 mm.

Slit strip and cut to length sheets are available upon request.

Mechanical Properties

Thickness
(mmin)
Thickness
(mmin)
2.00 - 3.000.079 - 0.118
Standard
SSAB
Coating
UC
Test direction
L
Yield strength ReH 1)
(min MPaksi)
65094
Tensile strength Rm
(MPaksi)
700 - 850101 - 123
Elongation A80 2)
(min %)
12
Elongation A5 3)
(min %)
14
Min. inner bending radius for a 90° bend 4)
(x t)
0.8
Thickness
(mmin)
Thickness
(mmin)
3.01 - 6.000.119 - 0.236
Standard
SSAB
Coating
UC
Test direction
L
Yield strength ReH 1)
(min MPaksi)
65094
Tensile strength Rm
(MPaksi)
700 - 850101 - 123
Elongation A80 2)
(min %)
—
Elongation A5 3)
(min %)
14
Min. inner bending radius for a 90° bend 4)
(x t)
1.2
Thickness
(mmin)
Thickness
(mmin)
6.01 - 10.000.237 - 0.393
Standard
SSAB
Coating
UC
Test direction
L
Yield strength ReH 1)
(min MPaksi)
65094
Tensile strength Rm
(MPaksi)
700 - 850101 - 123
Elongation A80 2)
(min %)
—
Elongation A5 3)
(min %)
14
Min. inner bending radius for a 90° bend 4)
(x t)
1.5

1) If ReH is not applicable then Rp0.2 is used. On thicknesses >8 mm the minimum yield strength may be 20 MPa lower.

2) A80 value applies for thicknesses < 3.00 mm.

3) A5 value applies for thicknesses ≥ 3.00 mm.

4) For both longitudinal and transverse direction.

 

Impact Properties

Product
Product
Docol S650MC D
Min. impact energy for longitudinal testing,
Charpy V 10x10 mm test specimen
40 J / -20 °C29 ft-lbs / -4 °F
Product
Product
Docol S650MC E
Min. impact energy for longitudinal testing,
Charpy V 10x10 mm test specimen
27 J / -40 °C20 ft-lbs / -40 °F
Impact testing according to EN ISO 148-1 is performed on thicknesses ≥ 6mm. The specified minimum value corresponds to a full-size specimen.

Chemical Composition (heat analysis)

C
(max %)
C
(max %)
0.12
Si
(max %)
0.21 1)
Mn
(max %)
2.00
P
(max %)
0.025
S
(max %)
0.010
Nb
(max %)
0.09 2)
V
(max %)
0.20 2)
Ti
(max %)
0.15 2)

1) If the material is to be hot-dip galvanized, this must be specified in the order. Galvanizing class A available upon request.

2) Sum of Nb, V and Ti = max 0.22%.

The steel is grain refined.

Carbon Equivalent CET(CEV)

Thickness (mmin)
Thickness (mmin)
Typ CET(CEV)
2.00 - 10.000.079 - 0.393
0.22 (0.34)

 

Tolerances

Hot rolled (UC): Tolerances in accordance to EN 10051.

Customized dimensional and shape tolerances are available upon request.

Surface Treatments

Uncoated (UC): available as black or pickled and oiled.

All surface treatments are in accordance with RoHS directive (2011/65/EU) and do not contain Chromium VI (Cr6+). Surface treatments provide only temporary surface protection during transportation and storage. In order to avoid corrosion damages, care must be taken to keep the products dry during transportation and storage. If they become wet, they must be separated and situated so that they are dried quickly.

Fabrication and Other Recommendations

For information concerning fabrication, see SSAB´s brochures on www.ssab.com or consult Tech Support.

Appropriate health and safety precautions must be taken when bending, welding, cutting, grinding or otherwise working on the products.

Docol® High Strength Low Alloy steel product offer

Docol® 420LA high strength low alloy

Ver producto

Docol HR100XF

Ver producto

Docol HR110XF

Ver producto

Docol® S600MC high strength low alloy

Ver producto

Docol® S650MC high strength low alloy

Ver producto

Docol® S700MC high strength low alloy

Ver producto

Docol® S900MC high strength low alloy

Ver producto

Docol S960MC

Ver producto

Docol® 460LA high strength low alloy

Ver producto

Docol® 500LA high strength low alloy

Ver producto

Docol® 550LA high strength low alloy

Ver producto

Docol® 600LA high strength low alloy

Ver producto

Docol® 650LA high strength low alloy

Ver producto

Docol® 700LA high strength low alloy

Ver producto

Contenido relacionado

Existencias de materiales de prueba

¿Desea descubrir aplicaciones únicas de automoción, probar nuevos métodos de producción o crear componentes más ligeros que ahorren combustible y mejoren la resistencia a los impactos y la sostenibilidad?

Más información

Datos de conformado para aceros AHSS Docol®

Los clientes existentes de Docol® disfrutan de un acceso 24/7 a los datos de conformado que necesita para ayudarle en su selección y simulación de aceros avanzados de alta resistencia para automoción.

Más información