Docol® S900MC high strength low alloy

Download data sheet

General Product Description

The high-strength structural steel Docol S900MC is a hot-rolled steel made for cold forming, with a minimum yield strength of 900 MPa. Docol S900MC meets or exceeds the requirements of S900MC in EN 10149-2. Docol S900MC is provided as cut-to-length sheets with excellent thickness accuracy and surface quality. Typical applications include a wide range of components and parts for lighter transport solutions.

Dimension Range

Docol S900MC is available as cut to length sheets with mill edge in thicknesses of 3.00 - 10.00 mm, widths up to 1600 mm and lengths up to 13 meters.

Mechanical Properties

Thickness
(mmin)
Thickness
(mmin)
3.00 - 8.000.118 - 0.315
Yield strength ReH 1)
(min MPa)
900
Tensile strength Rm
(MPa)
930 - 1200
Elongation A5
(min %)
8
Min. inner bending radius for a 90° bend 2)
(x t)
3.0
Thickness
(mmin)
Thickness
(mmin)
8.01 - 10.000.315 - 0.3937
Yield strength ReH 1)
(min MPa)
900
Tensile strength Rm
(MPa)
930 - 1200
Elongation A5
(min %)
8
Min. inner bending radius for a 90° bend 2)
(x t)
3.5

The mechanical properties are tested in the longitudinal direction.

1) If ReH is not applicable then Rp0.2 is used.

2) For both longitudinal and transverse direction.

 

Impact Properties

Product
Product
Docol S900MC
Min. impact energy for longitudinal testing,
Charpy V 10x10 mm test specimen 1)
27 J / -40 °C

1) Impact testing according to EN 10149-2 ( -20 °C /minimum 40J) is available if specified at the time of order.

Impact testing according to EN ISO 148-1 is performed on thicknesses ≥ 5mm. The specified minimum value corresponds to a full-size specimen.

Chemical Composition (heat analysis)

C
(max %)
C
(max %)
0.10
Si
(max %)
0.25
Mn
(max %)
1.30
P
(max %)
0.020
S
(max %)
0.010
Nb
(max %)
0.05 1)
V
(max %)
0.05 1)
Ti
(max %)
0.07 1)

1) Sum of Nb, V and Ti = max 0.22%.

The steel is grain refined.

Carbon Equivalent CET(CEV)

Thickness (mmin)
Thickness (mmin)
Typ CET(CEV)
3.00 - 7.990.118 - 0.315
0.25 (0.50)
8.00 - 10.000.315 - 0.3937
0.27 (0.53)

 

Tolerances

Hot rolled (UC): Tolerances in accordance to EN 10051.

Customized dimensional and shape tolerances are available upon request.

Surface Treatments

Uncoated (UC): available as rolled or pickled and oiled or pickled-dry. As pickled and oiled and pickled-dry up to 5mm thickness.

All surface treatments are in accordance with RoHS directive (2011/65/EU) and do not contain Chromium VI (Cr6+). Surface treatments provide only temporary surface protection during transportation and storage. In order to avoid corrosion damages, care must be taken to keep the products dry during transportation and storage. If they become wet, they must be separated and situated so that they are dried quickly.

Delivery Conditions

Docol S900MC is supplied in as rolled surface condition or as pickled surface condition. The product is thermomechanically rolled.

Fabrication and Other Recommendations

Welding, bending and machining

Docol S900MC has good welding, cold forming and cutting performance.

Docol S900MC is a cold forming steel not suited for use at temperatures above 400°C since the material may then lose its guaranteed properties.

For information concerning fabrication, see SSAB´s brochures on www.ssab.com or consult Tech Support.

Appropriate health and safety precautions must be taken when bending, welding, cutting, grinding or otherwise working on the products.

Docol® High Strength Low Alloy steel product offer

Docol® 420LA high strength low alloy

Ver producto

Docol HR100XF

Ver producto

Docol HR110XF

Ver producto

Docol® S600MC high strength low alloy

Ver producto

Docol® S650MC high strength low alloy

Ver producto

Docol® S700MC high strength low alloy

Ver producto

Docol® S900MC high strength low alloy

Ver producto

Docol S960MC

Ver producto

Docol® 460LA high strength low alloy

Ver producto

Docol® 500LA high strength low alloy

Ver producto

Docol® 550LA high strength low alloy

Ver producto

Docol® 600LA high strength low alloy

Ver producto

Docol® 650LA high strength low alloy

Ver producto

Docol® 700LA high strength low alloy

Ver producto

Contenido relacionado

Existencias de materiales de prueba

¿Desea descubrir aplicaciones únicas de automoción, probar nuevos métodos de producción o crear componentes más ligeros que ahorren combustible y mejoren la resistencia a los impactos y la sostenibilidad?

Más información

Datos de conformado para aceros AHSS Docol®

Los clientes existentes de Docol® disfrutan de un acceso 24/7 a los datos de conformado que necesita para ayudarle en su selección y simulación de aceros avanzados de alta resistencia para automoción.

Más información