Strenx® Tube 700MLH

Download data sheet

Select Language

Get datasheet by email
Close

Get datasheet by email

On this page

General Product Description

Strenx® Tube 700MLH is an HF-welded cold-formed structural hollow section made of hot-rolled high-strength steel with a minimum yield strength of 700 MPa.

Its high strength combined with naturally stiff form of welded hollow section enables construction of stronger and lighter structures. Strenx® Tube 700MLH meets or exceeds the requirements o EN 10219-3 (2020) and it is CE marked according to EN 1090-2. Typical applications include load-bearing structures in the lifting, handling and transportation segments, especiallyin conditions that require extremely good toughness.

Strenx® Tube 700MLH is available in circular, square and rectangular shapes. Other shapes and sizes are available upon request.

The maximum length of the tubes is 12-18 meters, depending on the size. Longer or cut-to-length tubes are available upon request.

Hot dip galvanizing Strenx® Tube 700MLH hollow sections maylead to cracking. Please consult SSAB Tech Support prior galvanization.

Dimension Range

Strenx® Tube 700MLH is available at circular, square and rectangular shapes.
Hide/Show specific columns Edit
Select columns to display
    Shapes Dimensions
    Circular (mmin) 42.4 - 323.91.669 - 12.752
    Square (mmin) 40x40 - 300x3001.575x1.575 - 11.811x11.811
    Rectangular (mmin) 50x30 - 400x2001.969x1.181 - 15.748x7.874
    Wall thickness (mmin) 2.0 - 10.00.079 - 0.393
    Mill length (mmin) 6000 - 12000 / 18000236.220 - 472.440 / 708.660
    Compare parameters

    Select one parameter to compare

    Comparison

      Shapes
      Circular (mmin)
      Dimensions
      42.4 - 323.91.669 - 12.752
      Shapes
      Square (mmin)
      Dimensions
      40x40 - 300x3001.575x1.575 - 11.811x11.811
      Shapes
      Rectangular (mmin)
      Dimensions
      50x30 - 400x2001.969x1.181 - 15.748x7.874
      Shapes
      Wall thickness (mmin)
      Dimensions
      2.0 - 10.00.079 - 0.393
      Shapes
      Mill length (mmin)
      Dimensions
      6000 - 12000 / 18000236.220 - 472.440 / 708.660

      Other shapes and sizes are available upon request. 

      Circular Dimensions

      Hide/Show specific columns Edit
      Select columns to display
        Outer diameter (mmin) 2.0 mm (kg/m) 3.0 mm (kg/m) 4.0 mm (kg/m) 5.0 mm (kg/m) 6.0 mm (kg/m) 8.0 mm (kg/m) 10.0 mm (kg/m)
        42.41.669 1.99
        48.31.902 2.28 3.35
        60.32.374 2.88 4.24 5.55
        76.12.996 5.41 7.11
        88.93.500 6.36 8.38 10.4
        101.64.000 7.29 9.63 11.9
        108.04.252 7.77 10.3 12.7
        114.34.500 8.23 10.9 13.5
        127.05.000 9.17 12.1 15.0
        139.75.500 13.4 16.6 19.8 26.0 32.0
        168.36.626 16.2 20.1 24.0 31.6 39.0
        219.18.626 26.4 31.5 41.7 51.6
        273.010.748 33.1 39.5 52.3 64.9
        323.912.752 47.0 62.3 77.4
        Compare parameters

        Select one parameter to compare

        Comparison

          Square Dimensions

          Hide/Show specific columns Edit
          Select columns to display
            Height x Width (mmin) 2.0 mm (kg/m) 3.0 mm (kg/m) 4.0 mm (kg/m) 5.0 mm (kg/m) 6.0 mm (kg/m) 8.0 mm (kg/m) 10.0 mm (kg/m)
            40 x 401.575 x 1.575 2.31 3.41
            50 x 501.969 x 1.969 2.93 4.38 5.45
            60 x 602.362 x 2.362 5.35 6.71
            70 x 702.756 x 2.756 6.33 7.97
            80 x 803.150 x 3.150 7.30 9.22 11.3
            90 x 903.543 x 3.543 8.27 10.5 12.8
            100 x 1003.937 x 3.937 9.25 11.7 14.4 17.0 21.4
            120 x 1204.724 x 4.724 14.3 17.6 20.8 26.4 31.8
            140 x 1405.512 x 5.512 16.8 20.7 24.5 31.4 38.1
            150 x 1505.906 x 5.906 18.0 22.3 26.4 34.0 41.3
            160 x 1606.299 x 6.299 19.3 23.8 28.3 36.5 44.4
            180 x 1807.087 x 7.087 27.0 32.1 41.5 50.7
            200 x 2007.874 x 7.874 30.1 35.8 46.5 57.0
            220 x 2208.661 x 8.661 39.6 51.5 63.2
            250 x 2509.843 x 9.843 45.2 59.1 72.7
            300 x 30011.811 x 11.811 71.6 88.4
            Compare parameters

            Select one parameter to compare

            Comparison

              Rectangular Dimensions

              Hide/Show specific columns Edit
              Select columns to display
                Height x Width (mmin) 2.0 mm (kg/m) 3.0 mm (kg/m) 4.0 mm (kg/m) 5.0 mm (kg/m) 6.0 mm (kg/m) 8.0 mm (kg/m) 10.0 mm (kg/m)
                50 x 301.969 x 1.181 2.41 3.41
                60 x 402.362 x 1.575 2.93 4.38 5.45
                80 x 403.150 x 1.575 5.35 6.71
                80 x 603.150 x 2.362 6.33 7.97
                100 x 503.937 x 1.969 6.81 8.59
                100 x 603.937 x 2.362 7.30 9.22 11.30
                100 x 803.937 x 3.150 8.27 10.5 12.8
                120 x 604.724 x 2.362 8.27 10.5 12.8
                120 x 804.724 x 3.150 9.25 11.7 14.4 17.0 21.4
                150 x 1005.906 x 3.937 14.9 18.3 21.7 27.7 33.4
                160 x 806.299 x 3.150 14.3 17.6 20.8 26.4
                180 x 1007.087 x 3.937 16.8 20.7 24.5 31.4 38.1
                200 x 1007.874 x 3.937 18.0 22.3 26.4 34.0 41.3
                200 x 1207.874 x 4.724 19.3 23.8 28.3 36.5 44.4
                250 x 1009.843 x 3.937 26.2 31.11 40.23 49.11
                250 x 1509.843 x 5.906 30.1 35.8 46.5 57.0
                260 x 18010.236 x 7.087 39.6 51.5 63.2
                300 x 20011.811 x 7.874 45.2 59.1 72.7
                400 x 20015.7480 x 7.874 71.6
                Compare parameters

                Select one parameter to compare

                Comparison

                  Mechanical Properties

                  Hide/Show specific columns Edit
                  Select columns to display
                    Yield strength Rp0.2
                    (min MPaksi)
                    Tensile strength Rm
                    (MPaksi)
                    Elongation A5 1)
                    (min %)
                    Strenx® Tube 700MLH 700101 750 - 950109 - 138 10
                    Compare parameters

                    Select one parameter to compare

                    Comparison

                      1) The hollow sections with D/T < 15 (round) or (B + H)/2T < 12,5 (rectangular and square), the minimum value of elongation is reduced by 2.

                      The mechanical properties for rectangular hollow sections are tested by SSAB on the longer side of the cross section.

                      Mechanical properties meet the requirements of EN 10219-3 (2020).

                      Impact Properties

                      Hide/Show specific columns Edit
                      Select columns to display
                        Product Min impact energy for transversal testing,
                        Charpy V 10x10 mm test specimen
                        Strenx® Tube 700MLH 27 J / -50 °C20 ft-lbs / -58 °F
                        Compare parameters

                        Select one parameter to compare

                        Comparison

                          Product
                          Strenx® Tube 700MLH
                          Min impact energy for transversal testing,
                          Charpy V 10x10 mm test specimen
                          27 J / -50 °C20 ft-lbs / -58 °F

                          1) Impact testing according to EN ISO 148-1 is performed on thicknesses ≥ 6 mm. The specified minimum value corresponds to a full-size specimen.

                          Chemical Composition (ladle analysis)

                          Hide/Show specific columns Edit
                          Select columns to display
                            C
                            (max %)
                            Si
                            (max %)
                            Mn
                            (max %)
                            P
                            (max %)
                            S
                            (max %)
                            Nb
                            (max %)
                            V
                            (max %)
                            Ti
                            (max %)
                            0.12 0.25 2.10 0.020 0.010 0.090 1) 0.20 1) 0.15 1)
                            Compare parameters

                            Select one parameter to compare

                            Comparison

                              1) Sum of Nb, V and Ti = max 0.22%

                              Chemical composition meets or exceeds the requirements of EN 10219-3 (2020).

                              In addition, boron (B), molybdenum (Mo), nickel (Ni) or copper (Cu) may be used as alloying elements either singly or in combination.

                              The steel is grain refined.

                              Carbon Equivalent CET(CEV)

                              Hide/Show specific columns Edit
                              Select columns to display
                                Wall Thickness (mm) 2.0 - 10.00.079 - 0.394
                                Typ CET(CEV) 0.24 (0.38)
                                Compare parameters

                                Select one parameter to compare

                                Comparison

                                  Wall Thickness (mm)
                                  Typ CET(CEV)
                                  2.0 - 10.00.079 - 0.394
                                  0.24 (0.38)

                                  Tolerance Circular

                                  Hide/Show specific columns Edit
                                  Select columns to display
                                    Characteristic Circular hollow sections
                                    Tolerances meet or exceed the requirements of EN 10219
                                    Outside diameter (D) (1 ±1%, with a minimum of ±0.5 mm and a maximum of ±10 mm
                                    Out-of-roundness 2%, when D/T ≤ 100
                                    Thickness (T) When D ≤ 323.9 mm: -5%/+10%, with a minimum of ±0.2 mm and maximum ±0.5 mm
                                    When 355.6 ≤ D ≤ 406.4 mm : ±10%, when T ≤ 5 mm / ±0.5 mm, when T > 5 mm
                                    When D > 406.4 mm : ±10%, with a maximum of ±2 mm
                                    Straightness 0.20% of total length and 3 mm over any 1 m length
                                    Mass per unit length Individual tube: ±6%
                                    Mill length 0/+50 mm, 6000 ≤ L ≤ 12000 - 18000 mm (standard lengths 6000 & 12000 mm)
                                    Exact length Agreed at the time of enquiry and order
                                    Compare parameters

                                    Select one parameter to compare

                                    Comparison

                                      Characteristic
                                      Outside diameter (D) (1
                                      Circular hollow sections
                                      Tolerances meet or exceed the requirements of EN 10219
                                      ±1%, with a minimum of ±0.5 mm and a maximum of ±10 mm
                                      Characteristic
                                      Out-of-roundness
                                      Circular hollow sections
                                      Tolerances meet or exceed the requirements of EN 10219
                                      2%, when D/T ≤ 100
                                      Characteristic
                                      Thickness (T)
                                      Circular hollow sections
                                      Tolerances meet or exceed the requirements of EN 10219
                                      When D ≤ 323.9 mm: -5%/+10%, with a minimum of ±0.2 mm and maximum ±0.5 mm
                                      When 355.6 ≤ D ≤ 406.4 mm : ±10%, when T ≤ 5 mm / ±0.5 mm, when T > 5 mm
                                      When D > 406.4 mm : ±10%, with a maximum of ±2 mm
                                      Characteristic
                                      Straightness
                                      Circular hollow sections
                                      Tolerances meet or exceed the requirements of EN 10219
                                      0.20% of total length and 3 mm over any 1 m length
                                      Characteristic
                                      Mass per unit length
                                      Circular hollow sections
                                      Tolerances meet or exceed the requirements of EN 10219
                                      Individual tube: ±6%
                                      Characteristic
                                      Mill length
                                      Circular hollow sections
                                      Tolerances meet or exceed the requirements of EN 10219
                                      0/+50 mm, 6000 ≤ L ≤ 12000 - 18000 mm (standard lengths 6000 & 12000 mm)
                                      Characteristic
                                      Exact length
                                      Circular hollow sections
                                      Tolerances meet or exceed the requirements of EN 10219
                                      Agreed at the time of enquiry and order

                                      1) All external dimensions are measured with a minimum distance from the end of the section. The distance must be a minimum of 100 mm.

                                      Tolerance Square

                                      Hide/Show specific columns Edit
                                      Select columns to display
                                        Characteristic Square hollow sections
                                        Tolerances meet or exceed the requirements of EN 10219
                                        Outside dimensions (B, H) 1) When B, H < 100 mm ±1 % minimum ±0.5 mm
                                        When 100 mm ≤ B, H ≤ 200 mm: ±0.8%
                                        When B, H > 200 mm: ±0.6%
                                        Thickness (T) -5% / +10 %, with a minimum of ±0.2 mm and maximum ±0.5 mm
                                        External corner profile When T ≤ 6 mm: 1.6 x T–2.4 x T
                                        When 6 mm < T ≤ 10 mm: 2.0 x T-3.0 x T
                                        When T > 10 mm: 2.4 x T–3.6 x T
                                        Squareness of side 90° ±1°
                                        Concavity/convexity 0.8%, with a minimum of 0.5 mm
                                        Twist 2 mm + 0.5 mm/m
                                        Straightness 0.15% of total length and 3 mm over any 1 m length
                                        Mass per unit length Individual tube: ±6%
                                        Mill length 0/+50 mm, 6000 ≤ L ≤ 12000 - 18000 mm (standard lengths 6000 & 12000 mm)
                                        Exact length Agreed at the time of enquiry and order
                                        Compare parameters

                                        Select one parameter to compare

                                        Comparison

                                          Characteristic
                                          Outside dimensions (B, H) 1)
                                          Square hollow sections
                                          Tolerances meet or exceed the requirements of EN 10219
                                          When B, H < 100 mm ±1 % minimum ±0.5 mm
                                          When 100 mm ≤ B, H ≤ 200 mm: ±0.8%
                                          When B, H > 200 mm: ±0.6%
                                          Characteristic
                                          Thickness (T)
                                          Square hollow sections
                                          Tolerances meet or exceed the requirements of EN 10219
                                          -5% / +10 %, with a minimum of ±0.2 mm and maximum ±0.5 mm
                                          Characteristic
                                          External corner profile
                                          Square hollow sections
                                          Tolerances meet or exceed the requirements of EN 10219
                                          When T ≤ 6 mm: 1.6 x T–2.4 x T
                                          When 6 mm < T ≤ 10 mm: 2.0 x T-3.0 x T
                                          When T > 10 mm: 2.4 x T–3.6 x T
                                          Characteristic
                                          Squareness of side
                                          Square hollow sections
                                          Tolerances meet or exceed the requirements of EN 10219
                                          90° ±1°
                                          Characteristic
                                          Concavity/convexity
                                          Square hollow sections
                                          Tolerances meet or exceed the requirements of EN 10219
                                          0.8%, with a minimum of 0.5 mm
                                          Characteristic
                                          Twist
                                          Square hollow sections
                                          Tolerances meet or exceed the requirements of EN 10219
                                          2 mm + 0.5 mm/m
                                          Characteristic
                                          Straightness
                                          Square hollow sections
                                          Tolerances meet or exceed the requirements of EN 10219
                                          0.15% of total length and 3 mm over any 1 m length
                                          Characteristic
                                          Mass per unit length
                                          Square hollow sections
                                          Tolerances meet or exceed the requirements of EN 10219
                                          Individual tube: ±6%
                                          Characteristic
                                          Mill length
                                          Square hollow sections
                                          Tolerances meet or exceed the requirements of EN 10219
                                          0/+50 mm, 6000 ≤ L ≤ 12000 - 18000 mm (standard lengths 6000 & 12000 mm)
                                          Characteristic
                                          Exact length
                                          Square hollow sections
                                          Tolerances meet or exceed the requirements of EN 10219
                                          Agreed at the time of enquiry and order

                                          1) All external dimensions are measured with a minimum distance from the end of the section. The distance must be a minimum of 100 mm.

                                          Tolerance Rectangular

                                          Hide/Show specific columns Edit
                                          Select columns to display
                                            Characteristic Rectangular hollow sections
                                            Tolerances meet or exceed the requirements of EN 10219
                                            Outside dimensions (B, H) 1) When B, H < 100 mm ±1 % minimum ±0.5 mm
                                            When 100 mm ≤ B, H ≤ 200 mm: ±0.8%
                                            When B, H > 200 mm: ±0.6%
                                            Thickness (T) -5% / +10 %, with a minimum of ±0.2 mm and maximum ±0.5 mm
                                            External corner profile When T ≤ 6 mm: 1.6 x T–2.4 x T
                                            When 6 mm < T ≤ 10 mm: 2.0 x T-3.0 x T
                                            When T > 10 mm: 2.4 x T–3.6 x T
                                            Squareness of side 90° ±1°
                                            Concavity/convexity 0.8%, with a minimum of 0.5 mm
                                            Twist 2 mm + 0.5 mm/m
                                            Straightness 0.15% of total length and 3 mm over any 1 m length
                                            Mass per unit length Individual tube: ±6%
                                            Mill length 0/+50 mm, 6000 ≤ L ≤ 12000 - 18000 mm (standard lengths 6000 & 12000 mm)
                                            Exact length Agreed at the time of enquiry and order
                                            Compare parameters

                                            Select one parameter to compare

                                            Comparison

                                              Characteristic
                                              Outside dimensions (B, H) 1)
                                              Rectangular hollow sections
                                              Tolerances meet or exceed the requirements of EN 10219
                                              When B, H < 100 mm ±1 % minimum ±0.5 mm
                                              When 100 mm ≤ B, H ≤ 200 mm: ±0.8%
                                              When B, H > 200 mm: ±0.6%
                                              Characteristic
                                              Thickness (T)
                                              Rectangular hollow sections
                                              Tolerances meet or exceed the requirements of EN 10219
                                              -5% / +10 %, with a minimum of ±0.2 mm and maximum ±0.5 mm
                                              Characteristic
                                              External corner profile
                                              Rectangular hollow sections
                                              Tolerances meet or exceed the requirements of EN 10219
                                              When T ≤ 6 mm: 1.6 x T–2.4 x T
                                              When 6 mm < T ≤ 10 mm: 2.0 x T-3.0 x T
                                              When T > 10 mm: 2.4 x T–3.6 x T
                                              Characteristic
                                              Squareness of side
                                              Rectangular hollow sections
                                              Tolerances meet or exceed the requirements of EN 10219
                                              90° ±1°
                                              Characteristic
                                              Concavity/convexity
                                              Rectangular hollow sections
                                              Tolerances meet or exceed the requirements of EN 10219
                                              0.8%, with a minimum of 0.5 mm
                                              Characteristic
                                              Twist
                                              Rectangular hollow sections
                                              Tolerances meet or exceed the requirements of EN 10219
                                              2 mm + 0.5 mm/m
                                              Characteristic
                                              Straightness
                                              Rectangular hollow sections
                                              Tolerances meet or exceed the requirements of EN 10219
                                              0.15% of total length and 3 mm over any 1 m length
                                              Characteristic
                                              Mass per unit length
                                              Rectangular hollow sections
                                              Tolerances meet or exceed the requirements of EN 10219
                                              Individual tube: ±6%
                                              Characteristic
                                              Mill length
                                              Rectangular hollow sections
                                              Tolerances meet or exceed the requirements of EN 10219
                                              0/+50 mm, 6000 ≤ L ≤ 12000 - 18000 mm (standard lengths 6000 & 12000 mm)
                                              Characteristic
                                              Exact length
                                              Rectangular hollow sections
                                              Tolerances meet or exceed the requirements of EN 10219
                                              Agreed at the time of enquiry and order

                                              1) All external dimensions are measured with a minimum distance from the end of the section. The distance must be a minimum of 100 mm.

                                              Delivery Conditions

                                              The tubes are cold formed and high frequency welded from thermomechanically rolled steel.