General Product Description

SSAB Domex 500MC Plus is a HSLA steel with enhanced toughness and local formability properties. The new generation HSLA steels are produced with carefully controlled production parameters resulting in a finer microstructure and low variation in the mechanical properties. Fine microstructure will significantly improve the cut edge quality, lead to improved local formability while still retaining an excellent global formability and improve the toughness.

Dimension Range

SSAB Domex 500MC Plus is available in thicknesses of 3.00-8.00 mm and widths up to 1800 mm as coils, slit coils and as cut to length in lengths up to 16 meters.

Mechanical Properties

Hide/Show specific columns Edit
Select columns to display
    Thickness
    (mmin)
    Yield strength ReH
    (min MPa)
    Tensile strength Rm
    (MPa)
    Elongation A80 1)
    (min %)
    Elongation A5 2)
    (min %)
    Min. inner bending radius for a 90° bend
    (x t)
    3.00 - 8.000.118 - 0.315 500 550 - 700 14 18 0.0
    Compare parameters

    Select one parameter to compare

    Comparison

      The mechanical properties are tested in the longitudinal direction.

      Bending properties for both longitudinal and transversal direction.

      1) A80 value applies for thicknesses < 3.00 mm.

      2) A5 value applies for thicknesses ≥ 3.00 mm.

      Impact Properties

      Hide/Show specific columns Edit
      Select columns to display
        Min. impact energy for longitudinal testing,
        Charpy V 10x10 mm test specimens
        40 J / -60 °C
        Compare parameters

        Select one parameter to compare

        Comparison

          Min. impact energy for longitudinal testing,
          Charpy V 10x10 mm test specimens
          40 J / -60 °C
          Impact testing according to EN ISO 148-1 is performed on thicknesses ≥ 6mm. The specified minimum value corresponds to a full-size specimen.

          Chemical Composition (ladle analysis)

          Hide/Show specific columns Edit
          Select columns to display
            C
            (max %)
            Si
            (max %)
            Mn
            (max %)
            P
            (max %)
            S
            (max %)
            Al
            (min %)
            Nb
            (max %)
            V
            (max %)
            Ti
            (max %)
            0.10 0.21 1) 1.60 0.025 0.010 0.015 0.09 2) 0.20 2) 0.15 2)
            Compare parameters

            Select one parameter to compare

            Comparison

              The steel is grain refined.

              1) SSAB Domex MC Si_only A

              2) The sum of Nb, V and Ti is max 0.22%.

              Carbon Equivalent

              Hide/Show specific columns Edit
              Select columns to display
                Thickness (mmin) 3.00 - 8.000.118 - 0.315
                Typical CEV (%) 0.30
                Typical CET (%) 0.21
                Compare parameters

                Select one parameter to compare

                Comparison

                  Thickness (mmin)
                  Typical CEV (%)
                  3.00 - 8.000.118 - 0.315
                  0.30
                  Thickness (mmin)
                  Typical CET (%)
                  3.00 - 8.000.118 - 0.315
                  0.21
                  CET and CEV formula

                  Tolerances

                  SSAB Domex is delivered with SSAB Domex tolerances, with improved guarantees compared to EN 10051. More details are available at SSAB.com

                  Thickness

                  SSAB Domex thickness tolerances correspond to 2/3 of EN 10051 as default value. After special agreement, tolerances down to 1/3 of EN 10051 can be delivered for certain products and dimensions.

                  Length and Width

                  SSAB Domex tolerances for width and length are according to SSAB standard and offer narrower width and length tolerances compared to EN 10051.

                  For coil and sheet with mill edge, the width tolerances are corresponding to -0/+20 mm.

                  For coil and sheet with cut edge, the width tolerances are corresponding to -0/+2 mm.

                  After special agreement, tighter tolerances can be delivered for certain products and dimensions. Length tolerances only apply for cut to length sheets.

                  Shape

                  According to EN 10051. Narrower tolerances are available on request.

                  Flatness

                  SSAB Domex tolerances guarantee a maximum flatness deviation of 3 mm/m in addition to the EN 10051 flatness requirements.

                  Flatness guarantees only apply for cut to length sheets.

                  Surface Properties

                  According to EN 10163-2 Class B, Subclass 3.

                  Delivery Conditions

                  Thermomechanically rolled.

                  Surface and edge condition

                  SSAB Domex MC products are available with non-pickled or pickled surface with mill or cut edge.

                  Fabrication and Other Recommendations

                  SSAB Domex MC are cold forming steels not suited for heat treatments at temperatures above 580°C, since the material may then lose its guaranteed properties.

                  SSAB Domex is well suited for all common thermal and mechanical cutting processes. SSAB Domex offers good cold forming properties. Welding can be performed, using all common methods and consumables.

                  For information concerning fabrication, see SSAB´s brochures on www.ssab.com or consult Tech Support.

                  Appropriate health and safety precautions must be taken when bending, welding, cutting, grinding or otherwise working on the products.

                  Contact Information

                  www.ssab.com/contact