SSAB Domex® 460MC

Download data sheet

Select Language

Get datasheet by email
Close

Get datasheet by email

On this page

General Product Description

SSAB Domex 460MC meets or exceeds the requirements of S460MC in EN 10149-2. Upon agreement, it can be delivered as dual certified. This dual certification will enable producers of steel structures, in accordance with EN 1090, to use SSAB Domex 460MC in their CE-marked final component or structure.

Dimension Range

SSAB Domex 460MC is available in thicknesses of 2.00-13.00 mm and widths up to 1800 mm as coils, slit coils and as cut to length in lengths up to 16 meters.

Mechanical Properties

Hide/Show specific columns Edit
Select columns to display
    Thickness
    (mmin)
    Yield strength ReH
    (min MPa)
    Tensile strength Rm
    (MPa)
    Elongation A80 1)
    (min %)
    Elongation A5 2)
    (min %)
    Min. inner bending radius for a 90° bend
    (x t)
    2.00 - 3.000.0787 - 0.118 460 520 - 670 15 19 0.5
    3.01 - 6.000.119 - 0.236 460 520 - 670 19 0.7
    6.01 - 13.000.237 - 0.5118 460 520 - 670 19 0.9
    Compare parameters

    Select one parameter to compare

    Comparison

      The mechanical properties are tested in the longitudinal direction.

      Bending properties for both longitudinal and transversal direction.

      1) A80 value applies for thicknesses < 3.00 mm.

      2) A5 value applies for thicknesses ≥ 3.00 mm.

      Impact Properties

      Hide/Show specific columns Edit
      Select columns to display
        Product Min. impact energy for longitudinal testing,
        Charpy V 10x10 mm test specimens
        SSAB Domex 460MC B
        SSAB Domex 460MC D 40 J / -20 °C
        SSAB Domex 460MC E 27 J / -40 °C
        Compare parameters

        Select one parameter to compare

        Comparison

          Product
          SSAB Domex 460MC B
          Min. impact energy for longitudinal testing,
          Charpy V 10x10 mm test specimens
          Product
          SSAB Domex 460MC D
          Min. impact energy for longitudinal testing,
          Charpy V 10x10 mm test specimens
          40 J / -20 °C
          Product
          SSAB Domex 460MC E
          Min. impact energy for longitudinal testing,
          Charpy V 10x10 mm test specimens
          27 J / -40 °C
          Impact testing according to EN ISO 148-1 is performed on thicknesses ≥ 6mm. The specified minimum value corresponds to a full-size specimen.

          Chemical Composition (ladle analysis)

          Hide/Show specific columns Edit
          Select columns to display
            C
            (max %)
            Si
            (max %)
            Mn
            (max %)
            P
            (max %)
            S
            (max %)
            Al
            (min %)
            Nb
            (max %)
            V
            (max %)
            Ti
            (max %)
            0.10 0.03 1) 1.50 0.025 0.010 0.015 0.09 2) 0.20 2) 0.15 2)
            Compare parameters

            Select one parameter to compare

            Comparison

              The steel is grain refined.

              1) Meets the requirements of category A (thin coatings) for hot-dip zinc-coating in EN 10149-2. Category B for thick coatings is available on request (Si 0.15-0.21%).

              2) The sum of Nb, V and Ti is max 0.22%.

              Carbon Equivalent

              Hide/Show specific columns Edit
              Select columns to display
                Thickness (mmin) 2.00 - 13.000.0787 - 0.5118
                Typical CEV (%) 0.29
                Typical CET (%) 0.20
                Compare parameters

                Select one parameter to compare

                Comparison

                  Thickness (mmin)
                  Typical CEV (%)
                  2.00 - 13.000.0787 - 0.5118
                  0.29
                  Thickness (mmin)
                  Typical CET (%)
                  2.00 - 13.000.0787 - 0.5118
                  0.20

                  Tolerances

                  SSAB Domex is delivered with SSAB Domex tolerances, with improved guarantees compared to EN 10051. More details are available at SSAB.com

                  Thickness

                  SSAB Domex thickness tolerances correspond to 2/3 of EN 10051 as default value. After special agreement, tolerances down to 1/3 of EN 10051 can be delivered for certain products and dimensions.

                  Length and Width

                  SSAB Domex tolerances for width and length are according to SSAB standard and offer narrower width and length tolerances compared to EN 10051.

                  For coil and sheet with mill edge, the width tolerances are corresponding to -0/+20 mm.

                  For coil and sheet with cut edge, the width tolerances are corresponding to -0/+2 mm.

                  After special agreement, tighter tolerances can be delivered for certain products and dimensions. Length tolerances only apply for cut to length sheets.

                  Shape

                  According to EN 10051. Narrower tolerances are available on request.

                  Flatness

                  SSAB Domex tolerances guarantee a maximum flatness deviation of 3 mm/m in addition to the EN 10051 flatness requirements.

                  Flatness guarantees only apply for cut to length sheets.

                  Surface Properties

                  According to EN 10163-2 Class A, Subclass 3.

                  Delivery Conditions

                  Thermomechanically rolled.

                  Surface and edge condition

                  SSAB Domex MC products are available with non-pickled or pickled surface with mill or cut edge.

                  Fabrication and Other Recommendations

                  SSAB Domex MC are cold forming steels not suited for heat treatments at temperatures above 580°C, since the material may then lose its guaranteed properties.

                  SSAB Domex is well suited for all common thermal and mechanical cutting processes. SSAB Domex offers good cold forming properties. Welding can be performed, using all common methods and consumables.

                  For information concerning fabrication, see SSAB´s brochures on www.ssab.com or consult Tech Support.

                  Appropriate health and safety precautions must be taken when bending, welding, cutting, grinding or otherwise working on the products.