A structural steel developed for use in demanding load-bearing structures within the Offshore and Marine Industry.
Strenx® 700 OME exceeds the requirements of S690QL, EN 10025-6. Strenx® 700 OME can be ordered with dual steel grades certificate, where the additional steel grade is defined and approved by one of the Classification Societies listed below. The dual certification offers You the benefits of excellent mechanical properties, extra tight tolerances, formability and consistency of SSAB Strenx® Guarantees.
| American Bureau of Shipping | AB EQ70 | 4.8 to 130 mm thickness |
| DNV - GL | NV E690, VL E690 | 6 to 80 mm thickness |
| Lloyds Register | LR EH 69 | 8 to 80 mm thickness |
For transverse test pieces.
Unless otherwise agreed, only transverse impact testing.
Option 1 - Min guaranteed impact energy (J) for transverse testing Charpy V 10x10 mm tests specimens 50 J/ -60 oC.
Option 2 - Improved deformation properties perpendicular to the surface. Through- thickness tensile testing according to EN 10 164, Class Z35, Z25 and Z15.
The steel is grain refined. *) Intentional alloying elements.
Tolerances according to Strenx® Thickness Guarantees.
Strenx® Guarantees meet the requirements of EN 10029 Class A, but offers narrower tolerances.
According to SSAB’s dimension program. Tolerances conform with EN 10029 or to SSAB’s standard after agreement.
Tolerances according to EN 10029.
Tolerances according to Strenx® Flatness Guarantee Class C, which are more narrow than EN 10029 Class N.
According to EN 10163-2 Class A, Subclass 3.
The delivery condition is Quenched and Tempered. The plates are delivered with sheared or thermally cut edges. Untrimmed edges after agreement.
Delivery requirements can be found in SSAB’s brochure Strenx® Guarantees or on www.ssab.com.
Recommendations are found in SSAB’s brochures at www.ssab.com or consult Tech Support.
Bendability according to Strenx® Bending Guarantee. Strenx® 700 OME has obtained its mechanical properties by quenching and subsequent tempering. The properties of the delivery condition cannot be retained after exposure to temperatures in excess of 580oC.
Appropriate health and safety precautions must be taken when welding, cutting, grinding or otherwise working on this product. Grinding, especially of primer coated plates, may produce dust with a high particle concentration.
Show specs in: