General Product Description

Docol HR100XF cold-forming steel is a thermomechanically rolled product with a minimum yield strength of 690 MPa. Docol HR100XF is a cold forming steel for light- and heavy transport solutions and components. Docol HR100XF meets the requirements of ASTM A1018 grade 100 and can be supplied according to A1018 specification on request.

Dimension Range

Docol HR100XF is available in thicknesses of 2.0 - 10.0 mm, and in widths up to 1600 mm as coil, slit coil and as cut to length sheets in lengths up to 16000 mm.

Mechanical Properties

Hide/Show specific columns Edit
Select columns to display
    Thickness
    (mmin)
    Yield strength ReH 1)
    (min MPaksi)
    Tensile strength Rm
    (min MPaksi)
    Elongation A50
    (min %)
    Docol HR100XF 2.00 - 10.000.079 - 0.393 690100 760110 12
    Compare parameters

    Select one parameter to compare

    Comparison

      The mechanical properties are tested in the transverse direction.

      1) If ReH is not applicable then Rp0.2 is used.

      Impact Properties

      Hide/Show specific columns Edit
      Select columns to display
        Product Min. impact energy for longitudinal testing,
        Charpy V 10x10 mm test specimen
        Docol HR100XF 27 J / -40 °C20 ft-lbs / -40 °F
        Compare parameters

        Select one parameter to compare

        Comparison

          Product
          Docol HR100XF
          Min. impact energy for longitudinal testing,
          Charpy V 10x10 mm test specimen
          27 J / -40 °C20 ft-lbs / -40 °F

          Bending Properties

          Hide/Show specific columns Edit
          Select columns to display
            Bending t < 3.48 mm 3.48 ≤ t ≤ 6.00 mm t > 6.00 mm
            Min. inner bending radius for a 90° bend 0.8 xt 1.2 xt 1.6 xt
            Compare parameters

            Select one parameter to compare

            Comparison

              Valid in both the longitudinal and transverse direction.

              Chemical Composition (ladle analysis)

              Hide/Show specific columns Edit
              Select columns to display
                C
                (max %)
                Si
                (max %)
                Mn
                (max %)
                P
                (max %)
                S
                (max %)
                Al
                (%)
                Ti
                (max %)
                Nb
                (max %)
                V
                (max %)
                Docol HR100XF 0.12 0.03 2.10 0.025 0.010 0.015 0.15 1) 0.09 1) 0.20 1)
                Compare parameters

                Select one parameter to compare

                Comparison

                  Docol HR100XF is available with different levels of Si: from max 0.03%, up to max 0.28%. Max Si 0.03% is the standard version that is suitable for hot dip galvanizing with thin Zinc layers, and for products that will not be galvanized. If the material is to be hot-dip galvanized and a thicker Zinc layer is requested, this must be specified at the time of order.

                  1) The sum of Nb, V and Ti is max 0.22%.

                  Tolerances

                  Thickness

                  Tolerances according to 1/2 of EN 10051 category D.

                  Length and Width

                  Tolerances according to EN 10051.

                  Shape

                  Tolerances according to EN 10051.

                  Flatness

                  Tolerance 3mm/m which only apply for cut to length sheets.

                  Surface Properties

                  According to EN 10163-2 Class A, Subclass 3.

                  Delivery Conditions

                  Thermomechanically Rolled. Docol HR100XF is available in as rolled or pickled surface condition with mill or cut edge.

                  Fabrication and Other Recommendations

                  Welding, bending and machining

                  Docol HR100XF has good welding, cold forming and cutting performance. Docol HR100XF is a cold forming steel not suited for heat treatments at temperatures above 580°C since the material then may lose its guaranteed properties.

                  For information concerning fabrication, see SSAB´s brochures on www.ssab.com or consult Tech Support.

                  Appropriate health and safety precautions must be taken when bending, welding, cutting, grinding or otherwise working on the products.