How to weld > Welding consumables

High strength, low-alloy consumables with yield strengths (Rₚ₀.₂) higher than 700 MPa

Strenx® performance steel 900–1300 types are frequently welded with consumables that have yield strengths of about 750–1100 MPa in the all-weld metal.

This group of consumables represents the highest strength available on the market. Their manufacturers do not normally specify preheat/interpass temperatures for these types of consumables.

The actual temperature can for example be determined in accordance with the European Norm EN 1011-2, Method B. In addition, SSAB has made its own general estimates of the lowest suitable preheat/interpass temperature in accordance with the table below. SSAB considers that the interpass temperature should be set at a maximum of +210 °C.

The permissible heat input follows our normal recommendations for the relevant steel grade.

Single plate thickness in the joint [mm]
Single plate thickness in the joint [mm]
  ≤ 10
Min. preheat temperature [°C]
 125
Single plate thickness in the joint [mm]
Single plate thickness in the joint [mm]
  10.1 – 20.0
Min. preheat temperature [°C]
 140 
Single plate thickness in the joint [mm]
Single plate thickness in the joint [mm]
 20.1 – 40.0
Min. preheat temperature [°C]
 175
Single plate thickness in the joint [mm]
Single plate thickness in the joint [mm]
 >40.0
Min. preheat temperature [°C]
 190

Estimated preheat levels for high strength consumables. SSAB does not take formal responsibility of these temperatures since they depend of the individual characteristics of the consumable being used.

Contact Technical support


The information in this report is only applicable to SSAB’s products and should not be applied to any other products than original SSAB products. 


This report provides general results and recommendations for SSAB steel products. This report is subject to SSAB’s Terms of Use. It shall be the user's responsibility to verify that the information contained herein is correct and is suitable to be used for the particular purpose and application of the user. The report is intended to be used by professional users only who possess adequate expertise, qualification and knowledge for the safe and correct use of the results and recommendations in this report. This report is provided “as is”. The use of the report is at user’s own discretion and risk and that users will be solely responsible for any use of this report. SSAB disclaims any liability for the content or potential errors of this report, including but not limited to warranties and condition of merchantability or fitness for a particular purpose or suitability for individual applications. SSAB shall not be liable for any kind of direct or indirect damages and/or costs related to or arising therefrom, whether special, incidental, consequential or directly or indirectly related to the use of, or the inability to use, the report or the content, information or results included therein. 

Copyright 2026