General Product Description

The Docol HR550Y600T HE steel is the next generation of hot-rolled high-strength low-alloy steels with improved local formability for higher edge ductility and cut-edge quality which leads to greatly improved hole expansion.

Docol HR550Y600T HE are especially suitable for operations where high strength in combination with demanding forming is needed where cut edges may limit the forming operation.

These next generation steels have a new and closely controlled production method resulting in a fine microstructure and steel and with excellent formability and cut-edge quality. The Docol HR550Y600T HE is less sensitive to tool-settings and -wear, and will deliver an improved cut-edge compared to conventional HSLA grades.

This grade is also well suited for forming and bending operations with a bend radius of 0xt and compared to a conventional HSLA grade, the typical hole expansion result is improved with approx. 30 percentage points.

Docol HR550Y600T HE will excel when optimizing any fine blanking, stamping or forming operation and will push the limit on how to utilize the benefits of steel.

Docol HR550Y600T HE can after agreement be adapted and delivered as dual certified with S550MC according to EN 10149-2.

Dimension Range

Docol HR550Y600T HE is available as Hot-rolled pickled and oiled coil, slit coils and cut to length sheets in thickness of 2.00*) - 7.00 mm and widths up to 1600 mm. Length up to 16 meters.

*)Some restrictions may occur, and will be handled on request.

Mechanical Properties

Docol HR550Y600T HE

Coating
UC
Yield strength Rp0.2
(min MPa)
550
Tensile strength Rm
(MPa)
610 - 750
Elongation A80 1)
(min %)
12
Elongation A5 2)
(min %)
16
Hole expansion ratio 3)
(% typical)
65
Min. inner bending radius for a 90° bend
0.0 x t

The mechanical properties are valid in the longitudinal direction.

Bending properties for both longitudinal and transversal direction.

1) A80 value applies for thicknesses < 3.00 mm.

2) A5 value applies for thicknesses ≥ 3.00 mm.

3) HER –ratio is average of three test results out of five tested samples by excluding minimum and maximum results.

Chemical Composition (ladle analysis)

Docol HR550Y600T HE

C
(max %)
0.12
Si
(max %)
0.03 1)
Mn
(max %)
1.80
P
(max %)
0.025
S
(max %)
0.010
Altot
(min %)
0.015
Nb
(max %)
0.09 2)
V
(max %)
0.20 2)
Ti
(max %)
0.15 2)

The steel is grain refined.

1) If the material is to be hot-dip galvanized, this must be specified in the order.

2) The sum of Nb, V and Ti is max 0.22%.

Tolerances

Hot-rolled (UC): Tolerances in accordance to EN 10051.

Customized dimensional and shape tolerances are available on request.

Fabrication and Other Recommendations

For information concerning fabrication, see SSAB´s brochures on www.ssab.com or consult Tech Support.

Appropriate health and safety precautions must be taken when bending, welding, cutting, grinding or otherwise working on the products.

Docol® High Edge Ductility steel product offer

Docol® 355HE high edge ductility

View product

Docol® 420HE high edge ductility

View product

Docol® 460HE high edge ductility

View product

Docol® 500HE high edge ductility

View product

Docol® 550HE high edge ductility

View product

Related content

AHSS trial material stock

Want to discover unique automotive applications for AHSS materials? Try new production methods? Or create lighter components that can improve fuel efficiency, crash-worthiness and sustainability?

Read more
car from above

Automotive steel applications

Docol® steel grades serve specific design purposes and are chosen by designers for a wide range of applications and used by OEMs and tier suppliers in millions of vehicles around the world.

Read more
Forming data for Docol® AHSS steels

Forming data for Docol® AHSS steels

Existing Docol® customers get 24/7 access to the forming data you need to help in your selection and simulation of automotive advanced high strength steels.

Read more
Copyright 2026