Trailer Design Guideline > Manufacturing

Welding heat input​

Strenx® hot-rolled high-strength structural steel

High-strength steels are somewhat sensitive to high heat inputs. Excessively high heat input de-creases the strength as well as the impact tough-ness of the welded joint. If the minimum yield strength of the base material must be achieved in the welded joint, the maximum recommended heat input should not exceed the values in the graph below.

Maximum recommended heat input (Q) for Strenx® 700MC in order to fulfill the minimum yield strength (Re) and impact toughness requirements at -40 °C.

The graph is valid for butt welds, welded with matching filler metal, and where the reinforcement has been removed before testing. The maximum interpass temperature is 100 °C. The  heat input can be calculated according to the formula:

Q = Heat input (kJ/mm)
k = Arc efficiency (-)
U = Voltage (V)
I = Current (A)
v = Travel speed (mm/min)

The arc efficiency values are 0.8 for MAG welding and 1.0 for SAW welding. If the weld is located in a low stressed area and the impact toughness requirement is of minor importance, higher heat inputs can be used.

Strenx® cold-rolled high-strength structural steel (CR)

Strenx® CR is produced in thinner gauges, making it more difficult to increase the heat power enough to limit the heat affected zone to a level that will allow for a failure of the base material. As a rule of thumb: weld with as low a heat input as possible.

Contact Technical support


The information in this report is only applicable to SSAB’s products and should not be applied to any other products than original SSAB products. 


This report provides general results and recommendations for SSAB steel products. This report is subject to SSAB’s Terms of Use. It shall be the user's responsibility to verify that the information contained herein is correct and is suitable to be used for the particular purpose and application of the user. The report is intended to be used by professional users only who possess adequate expertise, qualification and knowledge for the safe and correct use of the results and recommendations in this report. This report is provided “as is”. The use of the report is at user’s own discretion and risk and that users will be solely responsible for any use of this report. SSAB disclaims any liability for the content or potential errors of this report, including but not limited to warranties and condition of merchantability or fitness for a particular purpose or suitability for individual applications. SSAB shall not be liable for any kind of direct or indirect damages and/or costs related to or arising therefrom, whether special, incidental, consequential or directly or indirectly related to the use of, or the inability to use, the report or the content, information or results included therein. 

Copyright 2026