Trailer Design Guideline > Design

Typical upgrading

Strenx® 700MC is commonly used in lightweight solutions for trailer chassis.

Upgrading a trailer chassis from a S355 (grade 50) grade to Strenx® 700MC (Strenx® 110 XF) typically generates a weight reduction of about 30% for the chassis structural parts. However, depending on the chassis design, the weight reduction potential may be even higher, up to 50%. As an example, we have calculated the potential weight reduction of an existing 13.75-meter-long trailer main beam produced from a S355 (grade 50) steel grade by introducing Strenx® 700MC. The load-carrying capacity of the existing design has been determined and a matching alternative in Strenx® 700MC is suggested in the illustration and table below.

The total weight of the original main members manufactured from conventional steel is 1,085 kg, and the total weight of the upgraded alternative in Strenx® 700MC is 704 kg. This gives a weight re-duction of 381 kg, or 35.2%. These results should be considered as an example. Depending on the type of vehicle, specific requirements and design details, the upgrading potential may be less or greater compared to our example. The calculations only consider static load-carrying capacity, but serve as a good starting point in developing a lightweight chassis design.

The main beams of a conventionally designed trailer chassis have limitations in using a strength higher than Strenx® 700MC for structural strength. Exploring other chassis concepts is necessary to truly benefit from higher strength. For certain special trailers, however, higher grades like Strenx® 960 may make an appropriate choice. For flanges or profiles that are susceptible to wear or dents, such as the rear bumper, a higher strength steel like Strenx® 1100 or a wear-resistant steel like Hardox® 450 can be specified. For other parts of the chassis, such as floor members, cold-rolled steels like Strenx® 700 CR and Strenx® 960 CR offer significant weight reduction opportunities. These parts can be produced by bending and, for larger series, roll-forming or stamping. 

Lightweight solutions for matching load-carrying capacity and bending stiffness.
Overview of the cross-sectional properties and the weight reduction potential of a conventional main beam 1) and upgraded, lightweight alternatives 2) and 3) in Strenx® 700MC. 

Steel Grade 
1) Original design
 S355
2) Lightweight design
 Strenx® 700 MC
3) Lightweight design
 Strenx® 700 MC
Weight, m [kg/m]
1) Original design
 42
2) Lightweight design
 27
3) Lightweight design
 30
Bending Moment Capacity, M [kNm]
1) Original design
 286
2) Lightweight design
 306
3) Lightweight design
 369
Moment of Inertia, I [%]
1) Original design
 100
2) Lightweight design
 66
3) Lightweight design
 100
Section Modulus, W [%]
1) Original design
 100
2) Lightweight design
 64
3) Lightweight design
 81
Weight Reduction, WR [%]
1) Original design
 100
2) Lightweight design
 36
3) Lightweight design
 30

Contact Technical support


The information in this report is only applicable to SSAB’s products and should not be applied to any other products than original SSAB products. 


This report provides general results and recommendations for SSAB steel products. This report is subject to SSAB’s Terms of Use. It shall be the user's responsibility to verify that the information contained herein is correct and is suitable to be used for the particular purpose and application of the user. The report is intended to be used by professional users only who possess adequate expertise, qualification and knowledge for the safe and correct use of the results and recommendations in this report. This report is provided “as is”. The use of the report is at user’s own discretion and risk and that users will be solely responsible for any use of this report. SSAB disclaims any liability for the content or potential errors of this report, including but not limited to warranties and condition of merchantability or fitness for a particular purpose or suitability for individual applications. SSAB shall not be liable for any kind of direct or indirect damages and/or costs related to or arising therefrom, whether special, incidental, consequential or directly or indirectly related to the use of, or the inability to use, the report or the content, information or results included therein. 

Copyright 2026