Thickness, Flatness, Bending

Thickness guarantee

SSAB guarantees a maximum thickness variation within one plate and strip as specified in the tables below.

Strenx® thickness guarantee - plate

Thickness tolerances are according to SSAB´s thickness guarantee and are closer than those specified in EN 10029 except for thicknesses exceeding 80 mm, for which the tolerance range is according to standard.

Nominal thickness
(mm)
Thickness tolerances (mm)
        Min           Max    Within plate   
4.0 ≤ t < 5.0      -0.3      +0.3 0.4
 5.0 ≤ t < 8.0      -0.3      +0.4 0.5
 8.0 ≤- t < 15.0      -0.5      +0.4 0.6
 15.0 ≤ t < 25.0     -0.6      +0.4 0.6
 25.0 ≤ t < 40.0      -0.7      +0.8
 0.7
 40.0 ≤ t < 80.0     -0.9      +1.4 1.2

Other tolerances can be supplied upon special agreement. Please contact your local sales
representative for more information.

Strenx® thickness guarantee - hot rolled strip

Thickness tolerances are according to SSAB´s thickness guarantee and are closer than those specified in EN 10051 strip products. All values in the table conform to 1/2 EN Category D.

Nominal thickness
(mm)
Thickness tolerances for a nominal width w (mm)
w ≤ 12001200 < w ≤ 15001500 < w ≤ 1800
  t ≤ 2.00 ± 0.12 ± 0.13
 ± 0.14
2.00 < t ≤ 2.50 ± 0.12
 ± 0.14
 ± 0.16
2.50 < t ≤ 3.00 ± 0.14
 ± 0.15
 ± 0.17
 3.00 < t ≤ 4.00 ± 0.15
 ± 0.17
 ± 0.18
 4.00 < t ≤ 5.00 ± 0.17
 ± 0.18
 ± 0.19
5.00 < t ≤ 6.00
 ± 0.18
 ± 0.19
 ± 0.20
 6.00 < t ≤ 8.00
 ± 0.20
 ± 0.21
 ± 0.21
 8.00 < t ≤ 10.00
 ± 0.22
 ± 0.23
 ± 0.24
 10.00 < t ≤ 12.50
 ± 0.24
 ± 0.25
 ± 0.26
12.50 < t ≤ 15.00
 ± 0.26
 ± 0.26
 ± 0.28

Other tolerances can be supplied upon special agreement. Please contact your local sales
representative for more information.

Strenx® thickness guarantee - cold rolled strip

Thickness tolerances are according to SSAB´s thickness guarantee, which corresponds to 3/4 EN 10131 normal tolerances for cold rolled products.

Nominal thickness
(mm)
Thickness tolerances for a nominal width w (mm)
  w ≤ 1200  1200 < w ≤ 1500w > 1500  
 0.70 ≤ t ≤ 0.80
 ± 0.04
 ± 0.06
 ± 0.07
 0.80 < t ≤ 1.00
 ± 0.06
 ± 0.07
 ± 0.08
1.00 < t ≤ 1.20
 ± 0.07
 ± 0.08
 ± 0.09
1.20 < t ≤ 1.60
 ± 0.09
 ± 0.10
 ± 0.12
1.60 < t ≤ 2.00
 ± 0.12
 ± 0.12
 ± 0.14
2.00 < t ≤ 2.10
 ± 0.14
 ± 0.15
 ± 0.16

Other tolerances can be supplied upon special agreement. Please contact your local sales
representative for more information.

Flatness tolerance

SSAB has four classes of flatness tolerances for Strenx®, depending on type of product and material strength. All classes conform to, or are better than the relevant standards. The flatness tolerances for class C and D fulfill the requirements in EN 10029, class A fulfills both the requirements in EN 10051 and EN 10029, and class B fulfills the requirements in EN 10131.

ClassProduct  Nominal thickness (mm)  Flatness (mm/1m ruler)
Steel Flatness
  AStrenx® 600MC D/E
Strenx® 650MC D/E
Strenx® 100 XF
Strenx® 110 XF
Strenx® 700MC D/E
Strenx® 700MC Plus
Strenx® 700HR W
Strenx® 900MC
Strenx® 900 Plus
Strenx® 960MC
Strenx® 960 Plus
Strenx® 960 HR W
Strenx® 1100MC
 1.5 ≤ t ≤ 12.7 3
 BStrenx® 700 CR
Strenx® 700 CR W
Strenx® 960 CR
Strenx® 1100 CR
 0.7 ≤ t ≤ 2.1 6
 CStrenx® 100
Strenx® 700 E/F
Strenx® 700 OME
Strenx® P700
Strenx® 900 E/F
Strenx® 960 E/F
 4.0 ≤ t < 5.0 5
 5.0 ≤ t < 8.0 4
 8.0 ≤ t < 40.0 3
 40.0 ≤ t ≤ 160.0 3
 DStrenx® 1100 E/F
Strenx® 1300 E/F
 4.0 ≤ t < 5.0 7
 5.0 ≤ t < 6.0 5
 6.0 ≤ t < 20.0 4
 20.0 ≤ t ≤ 40.0 3

Class A is closer than EN 10051 and EN 10029.
Class B is closer than EN 10131 special tolerance class.
Classes C and D are closer than EN 10029 steel type L.
Short waves (300 - 1000 mm) according to EN 10029. In the case of discrepancies, the given class in the English version shall prevail.

Bending guarantee

Strenx® bending guarantee plate

SSAB has four bending guarantee classes for Strenx® plate according to the table below. The bending guarantees for Strenx® plate products are based on dies with rolls and normal friction (no lubrication). R/t stands for radius (R) divided by sheet thickness (t). These bending guarantees are based on bend tests of one step to 90° after unloading.

All classes conform to or are closer than the requirements in EN 10025-6. The bending guarantees also conform to and exceed the requirements in EN ISO 7438.

 ClassProduct  Nominal thickness
(t) (mm)
Guaranteed minimum final
inner radius on plate
Recommended initial punch radius
Die opening
width (W)
minimum W/t
 Ri/t transverse
to rolling
direction
 Ri/t along
rolling
direction
 Rp/t transverse
to rolling
direction
 Rp/t along
rolling
direction
  AStrenx® 100
Strenx® 700 E/F
Strenx® P700
Strenx® 700 OME
 t < 81.5 1.82.02.5 10
 8 ≤ t < 151.5 1.82.02.5 10
 15 ≤ t < 20
 1.7 2.1 2.0 2.5 12
 t ≥ 20
2.02.2 2.6 2.8 12
 BStrenx® 900 E/F
Strenx® 960 E/F
 t < 8 2.3 2.5 2.8 3.0 12
 8 ≤ t < 15 2.3 2.6 2.8 3.2 14
 15 ≤ t < 20
 2.4 2.7 2.8 3.2 14
 t ≥ 20
 2.8 3.4 3.0 3.5 16
  C Strenx® 1100 E/F t < 8 2.8 3.3 3.2 3.6 12
 8 ≤ t < 15 3.4 3.6 3.8 4.0 14
 15 ≤ t < 20  3.4 3.6 3.8 4.0 14
t ≥ 20
 3.7 4.0 4.2 4.5 16
 DStrenx® 1300 E/F t < 8 3.1 3.8 3.5 4.0 14
 8 ≤ t < 15 3.6 4.3 4.0 4.5 14

The guaranteed values for bending are valid under conditions given in the brochure Bending of Strenx®. In the case of discrepancies, the given class in the English version shall prevail.

Strenx® bending guarantee strip

SSAB has four bending guarantee classes for Strenx® plate according to the table below. The bending guarantees for Strenx® plate products are based on dies with rolls and normal friction (no lubrication). R/t stands for radius (R) divided by sheet thickness (t). These bending guarantees are based on bend tests of one step to 90° after unloading. Die opening widths are guidelines and may vary somewhat without affecting bending results.

Both Strenx® hot rolled and cold rolled strip steels have a guaranteed minimum bending radius valid for both longitudinal and transversal directions. For the hot rolled materials, the guarantees are closer than the requirements in EN 10149. The guaranteed values can also be found in respective data sheet.

Product Nominal thickness
(t) (mm)
Guaranteed minimum final
inner radius on sheet
Recommended minimum punch
radius to use
Die opening width (W)
min W/ts
 Ri/t transverse
to rolling
direction
 Ri/t along
rolling
direction
 Rp/t transverse
to rolling
direction
 Rp/t along
rolling
direction
 Strenx® 600MC D/Et ≤ 3.00.70.70.70.710
3.0 < t ≤ 6.01.11.11.11.110
 t > 6.01.41.41.41.410
Strenx® 650MC D/E
Strenx® 100 XF
 t ≤ 3.00.80.80.80.810
3.0 < t ≤ 6.01.21.21.21.210
t > 6.01.51.51.51.510

Strenx® 110 XF
Strenx® 700MC D/E
 t ≤ 3.00.80.81.01.010
3.0 < t ≤ 6.01.21.21.41.410
 t > 6.01.61.61.71.710
Strenx® 700 HR W3.0 ≤ t ≤ 6.01.21.21.41.410
 t > 6.01.61.61.71.710
Strenx® 700 MC Plus 3.0 ≤ t ≤ 10.0 1.01.01.31.310
 t > 10.01.51.51.81.810
 Strenx® 700 CR 0.7 ≤ t ≤ 2.12.02.02.52.510
 Strenx® 900MC 3.0 ≤ t ≤ 8.03.03.03.03.2512
 t > 8.03.53.53.53.7512
 Strenx® 900 Plus 2.0 ≤ t ≤ 8.03.03.04.04.012
 Strenx® 960MC 3.0 < t ≤ 10.03.53.53.64.012
 Strenx® 960 HR W 3.0 < t ≤ 6.13.53.54.04.012
  Strenx® 960 Plus  2.0 ≤ t ≤ 8.03.53.54.04.212
 Strenx® 960 CR 0.8 ≤ t ≤ 2.13.53.54.54.512
 Strenx® 1100MC3.0 ≤ t ≤ 8.04.04.04.75.014
Strenx® 1100 CR 0.8 ≤ t ≤ 2.13.53.54.54.514

The guaranteed values for bending are valid under conditions given in the brochure Bending of High Strength Steel. In the case of discrepancies, the given class in the English version shall prevail.

 