Tipper design > Dent resistance in tipper bodies

Tipper body impact tests

To better understand the dent resistance of different steel grades, SSAB built its own test rig. In the rig, different factors could be tested, such as the weight of the object to drop, plate thickness and free area as well as drop height, drop weight and tip radius.

The SSAB drop hammer test rig: a) Applied mass. b) Guide columns. c) Impactor. d) Drop height. e) Specimen between clamps. f) Laser beam.

 Drop height max.
 2.82 m (9.252’)
 Hammer weight
 180 - 400 kg (397 -  882 lbs.) 
 Impact radius
 30 - 50 mm (1.181 -  1.969”)
 Frame size opening
 500 x 500 or 800 x 800 mm (20 x 20” or 32 x 32”)
 Maximum test plate thickness
 50 mm (1.969”)

Parameters for the impact test rig.

Results from the drop hammer rig show that using Hardox® 500 Tuf instead of Hardox® 450 reduces dent depths. In some cases, even though a thinner plate of Hardox® 500 Tuf is used, it will dent less than Hardox® 450.

Drop hammer impact test for Hardox® 450 and Hardox® 500 Tuf. The dent depths are examples. Other factors, such as suspension and rock toughness, will also influence the dent resistance.

Contact Technical support


The information in this report is only applicable to SSAB’s products and should not be applied to any other products than original SSAB products. 


This report provides general results and recommendations for SSAB steel products. This report is subject to SSAB’s Terms of Use. It shall be the user's responsibility to verify that the information contained herein is correct and is suitable to be used for the particular purpose and application of the user. The report is intended to be used by professional users only who possess adequate expertise, qualification and knowledge for the safe and correct use of the results and recommendations in this report. This report is provided “as is”. The use of the report is at user’s own discretion and risk and that users will be solely responsible for any use of this report. SSAB disclaims any liability for the content or potential errors of this report, including but not limited to warranties and condition of merchantability or fitness for a particular purpose or suitability for individual applications. SSAB shall not be liable for any kind of direct or indirect damages and/or costs related to or arising therefrom, whether special, incidental, consequential or directly or indirectly related to the use of, or the inability to use, the report or the content, information or results included therein. 

Copyright 2026