Thickness, Flatness, Bending

Hardox® thickness guarantee

Hardox® thickness guarantee - plate

Thickness tolerances are according to SSAB´s thickness guarantee and are closer than those specified in EN 10029 (Class A), except for thicknesses exceeding 80 mm, for which the tolerance range is according to standard. The thickness shall be measured at any point situated more than 25 mm from the transverse or longitudinal edges of the plate.

Nominal thickness (mm)Thickness tolerances (mm)
MinMaxWithin plate
3.2 ≤ t < 5.0-0.3+0.30.4
5.0 ≤ t < 8.0-0.3+0.40.5
8.0 ≤ t < 15.0-0.5+0.40.6
15.0 ≤ t < 25.0-0.6+0.4
0.6
25.0 ≤ t < 40.0-0.7+0.80.7
40.0 ≤ t < 80.0-0.9+1.41.2
80.0 ≤ t ≤ 160.0-1.1+2.11.5

Other tolerances can be supplied upon special agreement.
Please contact your local sales representative for more information.

 

Hardox® thickness guarantee - hot rolled cut-to-length sheet

Thickness tolerances are according to SSAB´s thickness guarantee and are closer than those specified in EN 10051 for cut-to-length sheets. All values in the table conform to 1/2 EN Category D. The thickness shall be measured at any point situated more than 40 mm from the edges for product with mill edge and a minimum of 25 mm for product with trimmed edges.

Nominal thickness (mm)Thickness tolerances for a nominal width w (mm)
w ≤ 12001200 < w ≤ 15001500 < w ≤ 1800
t ≤ 2.00± 0.12± 0.13± 0.14
2.00 < t ≤ 2.50± 0.12± 0.14± 0.16
2.50 < t ≤ 3.00± 0.14± 0.15± 0.17
3.00 < t ≤ 4.00± 0.15± 0.17
± 0.18
4.00 < t ≤ 5.00± 0.17± 0.18± 0.19
5.00 < t ≤ 6.00± 0.18± 0.19± 0.20
6.00 < t ≤ 8.00± 0.20± 0.21± 0.21

Other tolerances can be supplied upon special agreement.
Please contact your local sales representative for more information.

 

Hardox® thickness guarantee - cold rolled cut-to-length sheet

Thickness tolerances are according to SSAB´s thickness guarantee, which corresponds to 3/4 EN 10131 normal tolerances for cold rolled cut-to-length sheets. The thickness shall be measured at any point located more than 40 mm from the edges.

Nominal thickness
(mm)
Thickness tolerances for a nominal width w (mm)
w ≤ 12001200 < w ≤ 1500
t ≤ 0.80± 0.04± 0.06
0.80 < t ≤ 1.00± 0.06± 0.07
1.00 < t ≤ 1.20± 0.07± 0.08
1.20 < t ≤ 1.60± 0.09± 0.10
1.60 < t ≤ 2.00± 0.12± 0.12
2.00 < t ≤ 2.10± 0.14± 0.16

Other tolerances can be supplied upon special agreement.
Please contact your local sales representative for more information.



Hardox® length and width guarantee

Hardox® length and width guarantee - plate

Length and width tolerances are according to those specified in EN 10029. According to EN 10029, the length of the plate is the length of the shorter of both longitudinal edges. The width shall be measured perpendicular to the major axis of the plate.

Nominal length (mm)Length tolerances (mm)
Min   Max   
l < 40000+ 20
4000 ≤ l < 60000+ 30
6000 ≤ l < 80000+ 40
8000 ≤ l < 100000+ 50
10000 ≤ l < 150000+ 75
15000 ≤ l ≤ 180000+ 100

 

Nominal thickness (mm)Width tolerances (mm)
MinMax
t < 400+ 20
40 ≤ t < 1500+ 25
150 ≤ t ≤ 1600+ 30

Mill edge tolerances upon request.
Please contact your local sales representative for more information.

 

Hardox® length and width guarantee – hot- and cold-rolled cut-to-length sheet

The length and width tolerances for Hardox® hot-rolled sheets exceed the tolerances given in EN 10051. The length and width tolerances for Hardox® cold-rolled sheets are according to the normal tolerances in EN 10131. The length of the sheet is the length of the shorter of both longitudinal edges. The width shall be measured at a right angles to the longitudinal axis of the product.

 

Length and width of hot-rolled sheet

Nominal length (mm)Length tolerances (mm)
LowerUpper
0 - 400003
4001 - 600004
6001 - 800005
8001 - 1300006
13001 - 1600008

 

Nominal width (mm)Width tolerances (mm)
Mill edgeTrimmed edges
LowerUpperLowerUpper
< 22000+ 200+ 2

 

Length and width of cold-rolled sheet

Nominal length (mm)Length tolerances (mm)
UnderOver
l < 20000+ 6
l ≥ 200000.3 % of the length

 

Nominal width (mm)Width tolerances (mm)
UnderOver
w ≤ 12000+ 4
1200 < w ≤ 15000+ 5
w > 15000+ 6


Hardox® flatness guarantee

SSAB has four classes of flatness tolerances for Hardox®, depending on type of product and hardness. All classes conform to or exceed the specifications in the relevant standards.

ClassProduct Nominal thickness (mm) Flatness (mm/1 m ruler)
steel flatness
AHardox® 400 sheet
Hardox® 400 sheet
Hardox® 450 sheet
Hardox® 500 sheet
Hardox® HiAce sheet
2.0 ≤ t ≤ 8.03
Hardox® 500 Tuf sheet2.5 ≤ t ≤ 8.0 
BHardox® 500 Tuf sheet 2.0 ≤ t < 2.56

Hardox® 450 CR sheet
Hardox® 600 sheet 

 0.8 ≤ t ≤ 6.0
CHardox® 400 plate
Hardox® 450 plate
Hardox® 500 plate
Hardox® 500 Tuf plate
Hardox® HiTemp plate
Hardox® HiAce plate
Hardox® HiTuf plate
3.2 ≤ t < 4.015
4.0 ≤ t < 5.07
5.0 ≤ t < 6.05
6.0 ≤ t < 20.0 4 
20.0 ≤ t ≤ 130.03
130.0 < t ≤ 160.04
DHardox® 550 plate
Hardox® 600 plate 
Hardox® Extreme plate
4.0 ≤ t ≤ 5.012
5.0 < t < 25.010
25.0 ≤ t < 40.09
40.0 ≤ t ≤ 65.08

Class A is closer than EN 10051.
Class B is closer than EN 10051 and EN 10131 special tolerances.
Class C is closer than EN 10029 steel type L (Class N), except for thicknesses < 4.0 mm.
Class D is according to EN 10029 steel type H.

Short waves (300-1000 mm) according to EN 10029.
In the case of discrepancies, the given class in the EN English version shall prevail.


Hardox® bending guarantee

SSAB has six bending guarantee classes for plate and cut-to-length sheets according to the table below. The bending guarantees for Hardox® wear plate and sheets are based on a dies with rolls and normal friction (no lubrication). These bend guarantees are based on bend tests of one step to 90° after unloading.

The bending guarantees conform to and exceed the requirements in EN ISO 7438. 

ClassProductNominal thickness (mm) Transverse to rolling direction minimum Rp/t
steel flatness
Along rolling direction minimum Rp/tDie opening width (W) minimum W/t
AHardox® 400 sheet
Hardox® 450 sheet
Hardox® HiAce sheet
Hardox® 500 Tuf sheet
2 ≤ t < 43.04.012
4 ≤ t ≤ 8 3.03.512
BHardox® 450 CR sheet0.8 ≤ t < 2.14.04.012
CHardox® 500 sheet2 ≤ t ≤ 7.03.54.012
D

Hardox® 400 plate

t < 82.53.012
8 ≤ t < 203.04.014
20 ≤ t < 504.05.016
EHardox® 450 plate
Hardox® 500Tuf plate
Hardox® HiTemp plate
Hardox® HiAce plate
3.2 ≤ t < 4.03.03.512
4.0 ≤ t < 5.03.54.514
5.0 ≤ t < 6.04.55.016
FHardox® 500 platet < 83.54.512
8 ≤ t < 154.04.514
15 ≤ t < 204.55.014
t ≥ 205.56.016

Rp/t stands for punch radius (Rp) divided by thickness (t). Die opening widths are guidelines and may vary somewhat without affecting bending results.

The guaranteed values for bending are valid under conditions given in the brochure Bending of Hardox® wear plate. In the case of discrepancies, the given class in the EN English version.