Duroxite® 100

Download data sheet

General Product Description

Duroxite® 100 is manufactured by depositing chromium-rich, abrasion-resistant materials on a mild steel base plate using a traditional arc welding process. The hardfacing overlay plate is suitable for severe abrasive wear and moderate to low impact applications. The multiple-layer overlay is also capable of maintaining full wear resistance up to 350 ºC (660ºF) and the typical surface hardness of 55 HRC at elevated temperatures up to 540°C (1000°F). Duroxite® 100 is available in single layers or multiple layers up to 20 mm (3/4”) in overlay thickness.

Key Benefits

  • Same wear resistance guaranteed from surface down to 75% of the overlay
  • Optimal carbide composition to provide good combination of wear resistance and homogenous bonding
  • Good formability due to staggered cracking pattern on overlay surface

Typical Applications

Standard Dimensions

Standard overlay thicknesses
Metric unit
Standard overlay thicknesses
Metric unit
3 mm on 6 mm
Standard overlay thicknesses
Metric unit
Standard overlay thicknesses
Metric unit
5 mm on 8 mm

Other plate sizes and custom thicknesses can be produced upon request.

Standard plate sizes

Metric unit
Metric unit
1.2 m x 2.4 m
Imperial unit
4' x 8'
Metric unit
Metric unit
1.4 m x 3.0 m
Imperial unit
4.6' x 10'
Metric unit
Metric unit
1.5 m x 3.0 m
Imperial unit
5' x 10'
Metric unit
Metric unit
1.8 m x 3.0 m
Imperial unit
6' x 10'
Metric unit
Metric unit
2.4 m x 3.0 m
Imperial unit
8' x 10'

Other plate sizes and custom thicknesses can be produced upon request.

Mechanical Properties

Single pass
ASTM G65 – Procedure A weight loss1)
Surface
(g max)
0.25
ASTM G65 – Procedure A weight loss1)
75 % depth of overlay2)
(g max)
0.25
Typical Bulk Surface Hardness
HRC
55 - 57
Typical Bulk Surface Hardness
HV
590 - 630
Double passes
ASTM G65 – Procedure A weight loss1)
Surface
(g max)
0.18
ASTM G65 – Procedure A weight loss1)
75 % depth of overlay2)
(g max)
0.18
Typical Bulk Surface Hardness
HRC
59 - 62
Typical Bulk Surface Hardness
HV
675 - 750
Triple and more passes
ASTM G65 – Procedure A weight loss1)
Surface
(g max)
0.18
ASTM G65 – Procedure A weight loss1)
75 % depth of overlay2)
(g max)
0.18
Typical Bulk Surface Hardness
HRC
60 - 64
Typical Bulk Surface Hardness
HV
700 - 810

Microstructure

The microstructure of Duroxite® 100 is composed of a high proportion of extremely hard primary M7C3 chromium-rich carbides with a typical hardness of 1700 HK*) dispersed evenly in a ductile eutectic austenite matrix. The volume fraction of primary carbides is maintained between 30 to 50% to provide a good combination of wear resistance and homogenous bonding. *)HK is the Knoop microhardness used primarily for very brittle materials.

Tolerances

More details are given in SSAB’s brochure Duroxite® Guarantees.

Thickness

Tolerances according to Duroxite® Thickness Guarantee.

Duroxite® overall and overlay thickness tolerances can be guaranteed within ±10% of specified thickness.

Flatness

Plate flatness tolerance can be guaranteed within ±3 mm (±1/8”) over 1.5 m (5’) plate length for plate dimensions equal to or less than 1.5 m (5’) x 3.0 m (10’). For plates greater than 1.5 m (5’) wide by 3.0 m (10’) long, the following flatness guarantees apply.

Standard overlay thicknesses
Metric unit
Standard overlay thicknesses
Metric unit
5 mm on 8 mm
Plate flatness tolerance guaranteed over 1.5m (5'),
Metric unit
1.8 m x 3.0 m
25 mm
Plate flatness tolerance guaranteed over 1.5m (5'),
Metric unit
2.4 m x 3.0 m
41 mm
Standard overlay thicknesses
Metric unit
Standard overlay thicknesses
Metric unit
6 mm on 6 mm
Plate flatness tolerance guaranteed over 1.5m (5'),
Metric unit
1.8 m x 3.0 m
25 mm
Plate flatness tolerance guaranteed over 1.5m (5'),
Metric unit
2.4 m x 3.0 m
38 mm
Standard overlay thicknesses
Metric unit
Standard overlay thicknesses
Metric unit
10 mm on 10 mm
Plate flatness tolerance guaranteed over 1.5m (5'),
Metric unit
1.8 m x 3.0 m
12 mm
Plate flatness tolerance guaranteed over 1.5m (5'),
Metric unit
2.4 m x 3.0 m
25 mm
Standard overlay thicknesses
Metric unit
Standard overlay thicknesses
Metric unit
12 mm on 12 mm
Plate flatness tolerance guaranteed over 1.5m (5'),
Metric unit
1.8 m x 3.0 m
6 mm
Plate flatness tolerance guaranteed over 1.5m (5'),
Metric unit
2.4 m x 3.0 m
16 mm

For custom sizes, please consult your local sales representative or Hardox Wearparts center for flatness guarantees.

Delivery Conditions

Duroxite® 100 is normally supplied in an as-welded condition, but can also be supplied in a ground condition upon request.

Fabrication and Other Recommendations

Welding, cutting, forming and machining

Recommendations can be found in the Duroxite® Product brochure, or consult your local technical support representative.

Bendability for Duroxite® overlay plate are according to Duroxite® Bending Guarantees.

Safety precautions

When welding or cutting Duroxite® products, gases and harmful fumes are produced that are chemically complex and difficult to classify. The major toxic component in the fumes is hexavalent chromium. The proper exhaust ventilation equipment and fume-extraction torches are recommended, as well as suitable protective clothing and respiratory protection for operators.