Docol® S700MC high strength low alloy

Download data sheet

General Product Description

The high-strength structural steel Docol S700MC is a hot-rolled steel made for cold forming, with a minimum yield strength of 700 MPa for stronger and lighter structures. Docol S700MC meets or exceeds the requirements of S700MC in EN 10149-2. Typical applications include a wide range of heavy trucks components and parts, such as frame rails and cross-members. Docol S700MC comes in coils, slit coils and cut-to-length sheets.

Dimension Range

Hot rolled / UC: thickness 2.00-10.00 mm, width up to 1600 mm.

Slit strip and cut to length sheets are available upon request.

Mechanical Properties

Thickness
(mmin)
Thickness
(mmin)
2.00 - 3.000.079 - 0.118
Standard
SSAB
Coating
UC
Test direction
L
Yield strength ReH 1)
(min MPaksi)
700101
Tensile strength Rm
(MPaksi)
750 - 950109 - 138
Elongation A80 2)
(min %)
10
Elongation A5 3)
(min %)
12
Min. inner bending radius for a 90° bend 4)
(x t)
0.8
Thickness
(mmin)
Thickness
(mmin)
3.01 - 6.000.119 - 0.236
Standard
SSAB
Coating
UC
Test direction
L
Yield strength ReH 1)
(min MPaksi)
700101
Tensile strength Rm
(MPaksi)
750 - 950109 - 138
Elongation A80 2)
(min %)
—
Elongation A5 3)
(min %)
12
Min. inner bending radius for a 90° bend 4)
(x t)
1.2
Thickness
(mmin)
Thickness
(mmin)
6.01 - 10.000.237 - 0.393
Standard
SSAB
Coating
UC
Test direction
L
Yield strength ReH 1)
(min MPaksi)
700101
Tensile strength Rm
(MPaksi)
750 - 950109 - 138
Elongation A80 2)
(min %)
—
Elongation A5 3)
(min %)
12
Min. inner bending radius for a 90° bend 4)
(x t)
1.6

1) If ReH is not applicable then Rp0.2 is used. On thicknesses >8 mm the minimum yield strength may be 20 MPa lower.

2) A80 value applies for thicknesses < 3.00 mm.

3) A5 value applies for thicknesses ≥ 3.00 mm.

4) For both longitudinal and transverse direction.

 

Impact Properties

Product
Product
Docol S700MC D
Min. impact energy for longitudinal testing,
Charpy V 10x10 mm test specimen
40 J / -20 °C29 ft-lbs / -4 °F
Product
Product
Docol S700MC E
Min. impact energy for longitudinal testing,
Charpy V 10x10 mm test specimen
27 J / -40 °C20 ft-lbs / -40 °F
Impact testing according to EN ISO 148-1 is performed on thicknesses ≥ 6mm. The specified minimum value corresponds to a full-size specimen.

Chemical Composition (heat analysis)

C
(max %)
C
(max %)
0.12
Si
(max %)
0.21 1)
Mn
(max %)
2.10
P
(max %)
0.020
S
(max %)
0.010
Nb
(max %)
0.09 2)
V
(max %)
0.20 2)
Ti
(max %)
0.15 2)

1) If the material is to be hot-dip galvanized, this must be specified in the order. Galvanizing class A available upon request.

2) Sum of Nb, V and Ti = max 0.22%.

The steel is grain refined.

Carbon Equivalent CET(CEV)

Thickness (mmin)
Thickness (mmin)
Typ CET(CEV)
2.00 - 10.000.079 - 0.393
0.25 (0.39)

 

Tolerances

Hot rolled (UC): Tolerances in accordance to EN 10051.

Customized dimensional and shape tolerances are available upon request.

Surface treatments

Uncoated (UC): available as black or pickled and oiled.

All surface treatments are in accordance with RoHS directive (2011/65/EU) and do not contain Chromium VI (Cr6+). Surface treatments provide only temporary surface protection during transportation and storage. In order to avoid corrosion damages, care must be taken to keep the products dry during transportation and storage. If they become wet, they must be separated and situated so that they are dried quickly.

Fabrication and Other Recommendations

For information concerning fabrication, see SSAB´s brochures on www.ssab.com or consult Tech Support.

Appropriate health and safety precautions must be taken when bending, welding, cutting, grinding or otherwise working on the products.

Docol® High Strength Low Alloy steel product offer

Docol® 420LA high strength low alloy

View product

Docol HR100XF

View product

Docol HR110XF

View product

Docol® S600MC high strength low alloy

View product

Docol® S650MC high strength low alloy

View product

Docol® S700MC high strength low alloy

View product

Docol® S900MC high strength low alloy

View product

Docol S960MC

View product

Docol® 460LA high strength low alloy

View product

Docol® 500LA high strength low alloy

View product

Docol® 550LA high strength low alloy

View product

Docol® 600LA high strength low alloy

View product

Docol® 650LA high strength low alloy

View product

Docol® 700LA high strength low alloy

View product

Related content

AHSS trial material stock

Want to discover unique automotive applications for AHSS materials? Try new production methods? Or create lighter components that can improve fuel efficiency, crash-worthiness and sustainability?

Read more

Automotive steel applications

Docol® steel grades serve specific design purposes and are chosen by designers for a wide range of applications and used by OEMs and tier suppliers in millions of vehicles around the world.

Read more