Docol® S900MC high strength low alloy

Download data sheet

General Product Description

The high-strength structural steel Docol S900MC is a hot-rolled steel made for cold forming, with a minimum yield strength of 900 MPa. Docol S900MC meets or exceeds the requirements of S900MC in EN 10149-2. Docol S900MC is provided as cut-to-length sheets with excellent thickness accuracy and surface quality. Typical applications include a wide range of components and parts for lighter transport solutions.

Dimension Range

Docol S900MC is available as cut to length sheets with mill edge in thicknesses of 3.00 - 10.00 mm, widths up to 1600 mm and lengths up to 13 meters.

Mechanical Properties

Thickness
(mm)
Thickness
(mm)
3.00 - 8.00
Yield strength ReH 1)
(min MPa)
900
Tensile strength Rm
(MPa)
930 - 1200
Elongation A5
(min %)
8
Min. inner bending radius for a 90° bend 2)
(x t)
3.0
Thickness
(mm)
Thickness
(mm)
8.01 - 10.00
Yield strength ReH 1)
(min MPa)
900
Tensile strength Rm
(MPa)
930 - 1200
Elongation A5
(min %)
8
Min. inner bending radius for a 90° bend 2)
(x t)
3.5

The mechanical properties are tested in the longitudinal direction.

1) If ReH is not applicable then Rp0.2 is used.

2) For both longitudinal and transverse direction.

 

Impact Properties

Product
Product
Docol S900MC
Min. impact energy for longitudinal testing,
Charpy V 10x10 mm test specimen 1)
27 J / -40 °C

1) Impact testing according to EN 10149-2 ( -20 °C /minimum 40J) is available if specified at the time of order.

Impact testing according to EN ISO 148-1 is performed on thicknesses ≥ 5mm. The specified minimum value corresponds to a full-size specimen.

Chemical Composition (heat analysis)

C
(max %)
C
(max %)
0.10
Si
(max %)
0.25
Mn
(max %)
1.30
P
(max %)
0.020
S
(max %)
0.010
Nb
(max %)
0.05 1)
V
(max %)
0.05 1)
Ti
(max %)
0.07 1)

1) Sum of Nb, V and Ti = max 0.22%.

The steel is grain refined.

Carbon Equivalent CET(CEV)

Thickness (mm)
Thickness (mm)
Typ CET(CEV)
3.00 - 7.99
0.25 (0.50)
8.00 - 10.00
0.27 (0.53)

 

Tolerances

Hot rolled (UC): Tolerances in accordance to EN 10051.

Customized dimensional and shape tolerances are available upon request.

Thickness

According to 1/2 of EN 10051 category D.

Length and Width

The width tolerances -0/+20 mm with mill edges and the length tolerances -0/+8mm as a maximum.

Shape

Tolerances according to EN 10051.

Flatness

≤ 3 mm/m flatness guarantee apply for cut to length sheets. 

Surface Properties

According to EN 10163-2 Class A, Subclass 3.

Surface Treatments

Uncoated (UC): available as rolled or pickled and oiled or pickled-dry. As pickled and oiled and pickled-dry up to 5mm thickness.

All surface treatments are in accordance with RoHS directive (2011/65/EU) and do not contain Chromium VI (Cr6+). Surface treatments provide only temporary surface protection during transportation and storage. In order to avoid corrosion damages, care must be taken to keep the products dry during transportation and storage. If they become wet, they must be separated and situated so that they are dried quickly.

Delivery Conditions

Docol S900MC is supplied in as rolled surface condition or as pickled surface condition. The product is thermomechanically rolled.

Fabrication and Other Recommendations

Welding, bending and machining

Docol S900MC has good welding, cold forming and cutting performance.

Docol S900MC is a cold forming steel not suited for use at temperatures above 400°C since the material may then lose its guaranteed properties.

For information concerning fabrication, see SSAB´s brochures on www.ssab.com or consult Tech Support.

Appropriate health and safety precautions must be taken when bending, welding, cutting, grinding or otherwise working on the products.

Docol® High Strength Low Alloy steel product offer

Docol® 420LA high strength low alloy

View product

Docol HR100XF

View product

Docol HR110XF

View product

Docol® S600MC high strength low alloy

View product

Docol® S650MC high strength low alloy

View product

Docol® S700MC high strength low alloy

View product

Docol® S900MC high strength low alloy

View product

Docol S960MC

View product

Docol® 460LA high strength low alloy

View product

Docol® 500LA high strength low alloy

View product

Docol® 550LA high strength low alloy

View product

Docol® 600LA high strength low alloy

View product

Docol® 650LA high strength low alloy

View product

Docol® 700LA high strength low alloy

View product

Related content

AHSS trial material stock

Want to discover unique automotive applications for AHSS materials? Try new production methods? Or create lighter components that can improve fuel efficiency, crash-worthiness and sustainability?

Read more

Automotive steel applications

Docol® steel grades serve specific design purposes and are chosen by designers for a wide range of applications and used by OEMs and tier suppliers in millions of vehicles around the world.

Read more

Forming data for Docol® AHSS steels

Existing Docol® customers get 24/7 access to the forming data you need to help in your selection and simulation of automotive advanced high strength steels.

Read more