GreenCoat RWS Pural BT color coated steel is available in matt finish. It uses a patented bio-based coating with Swedish rapeseed oil, which is unique on the market. SSAB holds a worldwide patent for this coating technology (Bio-based Technology, BT).

GreenCoat RWS Pural BT offers the highest level of durability for rainwater systems using a double-sided coating (same coating is applied on both sides of the sheet).

GreenCoat RWS Pural BT color coated steel provides excellent corrosion resistance (RC5), gloss retention and color fastness (Ruv5). GreenCoat RWS Pural BT possesses excellent forming properties enabling very demanding folding even down to -15°C, allowing for year round installation at lower costs.

Excellent weather resistance together with regular maintenance and the cleaning of rainwater systems can maximize the service life of the product.

GreenCoat RWS Pural BT complies with current REACH regulations and is fully chromate-free.

SSAB’s color coated steels are all manufactured according to EN 10169.

GreenCoat and Pural are trademarks of the SSAB group of companies.

Technical Properties

Hide/Show specific columns Edit
Select columns to display
    Technical Properties Matt
    Gloss < 5
    Minimum inner bending radius 0.5 x sheet thickness
    Scratch resistance 30 N
    Lowest forming temperature -15 °C
    UV radiation resistance RUV5
    Corrosion resistance 1) RC5
    Stain resistance Good
    Highest operating temperature 100 °C
    Coating thickness, nominal (primer + top coat) 40 µm
    Coating structure Structured and wrinkled
    Steel designation 2) PLX , FAX , S280GD, DX51D, DX52D/RWS , DX54D 3)
    Zinc coating 275 g/m2
    Min steel thickness 2) 0.50 mm
    Steel width 2) 1000 - 1500 mm 4)
    Compare parameters

    Select one parameter to compare

    Comparison

      Technical Properties
      Gloss
      Matt
      < 5
      Technical Properties
      Minimum inner bending radius
      Matt
      0.5 x sheet thickness
      Technical Properties
      Scratch resistance
      Matt
      30 N
      Technical Properties
      Lowest forming temperature
      Matt
      -15 °C
      Technical Properties
      UV radiation resistance
      Matt
      RUV5
      Technical Properties
      Corrosion resistance 1)
      Matt
      RC5
      Technical Properties
      Stain resistance
      Matt
      Good
      Technical Properties
      Highest operating temperature
      Matt
      100 °C
      Technical Properties
      Coating thickness, nominal (primer + top coat)
      Matt
      40 µm
      Technical Properties
      Coating structure
      Matt
      Structured and wrinkled
      Technical Properties
      Steel designation 2)
      Matt
      PLX , FAX , S280GD, DX51D, DX52D/RWS , DX54D 3)
      Technical Properties
      Zinc coating
      Matt
      275 g/m2
      Technical Properties
      Min steel thickness 2)
      Matt
      0.50 mm
      Technical Properties
      Steel width 2)
      Matt
      1000 - 1500 mm 4)

      1) Classification into corrosion resistance categories is based on blistering, delamination and damage on bend of the coating after two years exposure in natural outdoor testing sites as specified in EN 10169.

      2) Maximum steel thickness is 1.5 mm and maximum steel width depends on steel thickness. For other steel dimensions or steel grades please contact SSAB Tech Support.

      3) FAX fulfills the requirements of EN 10346 DX51D, PLX fulfills the requirements of EN 10346 DX54D, DX52D/RWS fulfills the requirements of EN 10346 DX52D.

      4) Max width 1420 mm for color RR33 / SS0015.

      Colors

      Colors shown in the color table are only indicative. To see the real visual appearance of the product, please order a color sample. Please note also that the same colors between the products may differ.
      5 Available Colors
      Preview colors
      Close

      Colors

      GreenCoat RWS Pural BT

      Mountain Grey

      RR23 / SS0036

      Matt

      Slate Grey

      RR2H3 / SS0534

      Matt

      Nordic Night Black

      RR33 / SS0015

      Matt

      Walnut Brown

      RR32 / SS0387

      Matt

      Chestnut Brown

      RR887 / SS0435

      Matt

      The product may have slight tonal difference between batches and especially if their time of production differs significantly.

      Reverse Side Coating

      Coating is applied in same color on both sides of the sheet.

      The technical properties apply for both sides. However, different sides of the sheet cannot be mixed due to the possibility of a visual difference. The reverse side may show wider variation in color and gloss.

      Reverse side stamping is not applicable for double sided products.

      Contact Information

      www.ssab.com/contact