    General Product Description

    DNV Grades NV A32, NV D32, and NV E32 are high-strength structural steels with a minimum specified yield strength of 46 ksi and specified minimum Charpy V-notch impact toughness properties.

    Applications

    Typical applications include shipbuilding and mobile offshore drilling units and structures.

    Available Dimensions

    Hide/Show specific columns Edit
    Select columns to display
      Grade Product type Thickness
      (inmm)
      Width
      (inmm)
      Length
      (inmm)
      NV A32 Plate 0.1969 - 5.915.001 - 150 75 - 129.91900 - 3299 79 - 9062000 - 23000
      NV D32 Plate 0.1969 - 5.915.001 - 150 75 - 129.91900 - 3299 79 - 9062000 - 23000
      NV E32 Plate 0.1969 - 5.915.001 - 150 75 - 129.91900 - 3299 79 - 9062000 - 23000
      Compare parameters

      Select one parameter to compare

      Comparison

        Width: Please inquire for plate widths less than 75 in. and plate widths greater than 129.9 in.

        Mechanical Properties

        Tensile testing is performed in the transverse direction.

        Hide/Show specific columns Edit
        Select columns to display
          Grade Thickness
          (inmm)
          Yield strength
          (min ksi)
          Tensile strength
          (ksi)
          Elongation A5 1)
          (min %)
          NV A32 0.1969 - 5.915.001 - 150 46 64 - 82 22
          NV D32 0.1969 - 5.915.001 - 150 46 64 - 82 22
          NV E32 0.1969 - 5.915.001 - 150 46 64 - 82 22
          Compare parameters

          Select one parameter to compare

          Comparison

            1) See DNV Rules for elongation requirements for alternative tensile specimens.

            Impact Properties

            Hide/Show specific columns Edit
            Select columns to display
              Grade Thickness
              (inmm)
              Test temperature
              (°F)
              Min Longitudinal Average Energy 1)
              (ft-lbs)
              NV A32 0.1969 - 2.005.001 - 50.8 32 23
              NV A32 2.01 - 2.7551.1 - 69.8 32 28
              NV A32 2.76 - 5.9170.1 - 150 32 34
              NV D32 0.1969 - 2.005.001 - 50.8 -4 23
              NV D32 2.01 - 2.7551.1 - 69.8 -4 28
              NV D32 2.76 - 5.9170.1 - 150 -4 34
              NV E32 0.1969 - 2.005.001 - 50.8 -40 23
              NV E32 2.01 - 2.7551.1 - 69.8 -40 28
              NV E32 2.76 - 5.9170.1 - 150 -40 34
              Compare parameters

              Select one parameter to compare

              Comparison

                1) Tests are to be taken in the longitudinal direction. Normally, transverse test specimens are not required unless otherwise specified in the order. Impact tests not required when material thickness is less than 0.236 in. unless otherwise specified.

                No more than one value below the specified miniminum average energy but no less than 70% of the specfied minimum average energy value.

                Minimum average energy for full-size specimens. Refer to DNV Rules for sub-size specimen energy requirements.

                Carbon Equivalent

                Hide/Show specific columns Edit
                Select columns to display
                  Grade NV A32 NV A32 NV A32 NV D32 NV D32 NV D32 NV E32 NV E32 NV E32
                  Thickness (inmm) 0.1969 - 2.005.001 - 50.8 2.001 - 4.0050.83 - 102 4.01 - 5.91102 - 150 0.1969 - 2.005.001 - 50.8 2.01 - 4.0051.1 - 102 4.01 - 5.91102 - 150 0.1969 - 2.005.001 - 50.8 2.01 - 4.0051.1 - 102 4.01 - 5.91102 - 150
                  CEV 1) (max wt %) 0.36 0.38 0.40 0.36 0.38 0.40 0.36 0.38 0.40
                  Compare parameters

                  Select one parameter to compare

                  Comparison

                    1) Carbon equivalent requirements for TMCP condition of supply only.