Thickness, Flatness, Bending

Thickness guarantee

SSAB guarantees a maximum thickness variation within one plate and strip as specified in the tables below.

Strenx® thickness guarantee - plate

Thickness tolerances are according to SSAB´s thickness guarantee and are closer than those specified in EN 10029 except for thicknesses exceeding 80 mm, for which the tolerance range is according to standard.

 Nominal thickness (mm) Thickness tolerances (mm)
          Min            Max     Within plate   
4.0 ≤ t < 5.0       -0.3       +0.3  0.4
 5.0 ≤ t < 8.0       -0.3       +0.4  0.5
 8.0 ≤- t < 15.0       -0.5       +0.4  0.6
 15.0 ≤ t < 25.0      -0.6       +0.4  0.6
 25.0 ≤ t < 40.0       -0.7       +0.8
 0.7
 40.0 ≤ t < 80.0      -0.9       +1.4  1.2
 80.0 ≤ t < 160.0      -1.1       +2.1  1.5

Other tolerances can be supplied upon special agreement. Please contact your local sales
representative for more information.

Strenx® thickness guarantee - hot rolled strip

Thickness tolerances are according to SSAB´s thickness guarantee and are closer than those specified in EN 10051 strip products. All values in the table conform to 1/2 EN Category D.

Nominal   thickness  Thickness tolerances for a nominal width w (mm)
(mm) w ≤ 1200 1200 < w ≤ 1500 1500 < w ≤ 1800
            t ≤ 2.00  ± 0.12  ± 0.13
 ± 0.14
2.00 < t ≤ 2.50  ± 0.12
 ± 0.14
 ± 0.16
2.50 < t ≤ 3.00  ± 0.14
 ± 0.15
 ± 0.17
 3.00 < t ≤ 4.00  ± 0.15
 ± 0.17
 ± 0.18
 4.00 < t ≤ 5.00  ± 0.17
 ± 0.18
 ± 0.19
5.00 < t ≤ 6.00
 ± 0.18
 ± 0.19
 ± 0.20
 6.00 < t ≤ 8.00
 ± 0.20
 ± 0.21
 ± 0.21
 8.00 < t ≤ 10.00
 ± 0.22
 ± 0.23
 ± 0.24
 10.00 < t ≤ 12.50
 ± 0.24
 ± 0.25
 ± 0.26
12.50 < t ≤ 15.00
 ± 0.26
 ± 0.26
 ± 0.28

Other tolerances can be supplied upon special agreement. Please contact your local sales
representative for more information.

Strenx® thickness guarantee - cold rolled strip

Thickness tolerances are according to SSAB´s thickness guarantee, which corresponds to 3/4 EN 10131 normal tolerances for cold rolled products.

 Nominal thickness (mm) Thickness tolerances for a nominal width w (mm)
    w ≤ 1200   1200 < w ≤ 1500 w > 1500  
 0.70 ≤ t ≤ 0.80
 ± 0.04
 ± 0.06
 ± 0.07
 0.80 < t ≤ 1.00
 ± 0.06
 ± 0.07
 ± 0.08
1.00 < t ≤ 1.20
 ± 0.07
 ± 0.08
 ± 0.09
1.20 < t ≤ 1.60
 ± 0.09
 ± 0.10
 ± 0.12
1.60 < t ≤ 2.00
 ± 0.12
 ± 0.12
 ± 0.14
2.00 < t ≤ 2.10
 ± 0.14
 ± 0.15
 ± 0.16

Other tolerances can be supplied upon special agreement. Please contact your local sales
representative for more information.

Flatness tolerance

SSAB has four classes of flatness tolerances for Strenx®, depending on type of product and material strength. All classes conform to or exceed the specifications in the relevant standards. The flatness tolerances for class C and D fulfill the requirements in EN 10029, class A fulfills both the requirements in EN 10051 and EN 10029, and class B fulfills the requirements in EN 10131.

Class Product   Nominal thickness (mm)
 Flatness (mm/1m ruler)
Steel Flatness
 A Strenx® 600MC D/E
Strenx® 650MC D/E
Strenx® 100 XF
Strenx® 110 XF
Strenx® 700MC D/E
Strenx® 700MC Plus
Strenx® 900MC
Strenx® 900 Plus
Strenx® 960MC
Strenx® 960 Plus
Strenx® 1100MC
Strenx® 1100 Plus
 1.5 ≤ t ≤ 12.7  3
 B Strenx® 700 CR
Strenx® 960 CR
Strenx® 1100 CR
 0.7 ≤ t ≤ 2.1  6
 C Strenx® 100
Strenx® 700 E/F
Strenx® 700 OME
Strenx® 900 E/F
Strenx® 960 E/F
 4.0 ≤ t < 5.0  5
 5.0 ≤ t < 8.0  4
 8.0 ≤ t < 40.0  3
 40.0 ≤ t ≤ 160.0  3
 D Strenx® 1100 E/F
Strenx® 1300 E/F
 4.0 ≤ t < 5.0  7
 5.0 ≤ t < 6.0  5
 6.0 ≤ t < 20.0  4
 20.0 ≤ t ≤ 40.0  3
 

Class A is closer than EN 10051 and EN 10029.
Class B is closer than EN 10131 special tolerance class.
Classes C and D are closer than EN 10029 steel type L.
Short waves (300 - 1000 mm) according to EN 10029. In the case of discrepancies, the given class in the English version shall prevail.

Bending guarantee

SSAB has four bending guarantee classes for plate according to the chart below. Information on which class applies to each grade is provided in the respective data sheet. All classes conform to or are closer than the requirements in EN 10 025-6. The bending guarantees also conform to EN ISO 7438.

Strenx™ MC steels have a guaranteed minimum bending radius, valid for both longitudinal and transversal directions, that is closer than standard EN 10 149. Check the data sheet for guaranteed values.

Strenx™ CR steels have a guaranteed minimum bending radius, valid for both longitudinal and transversal directions. Check the data sheet for guaranteed values.

 Class  Nominal thickness
 Punch radius minimum R/t (1)
Bending direction (2)

            ┴                         ║

  A  t < 8  1.5  2.0
 8 ≤ t < 15  1.5  2.0
 15 ≤ t < 20
 2.0  2.5
 t 20
 2.0  2.5
 B  t < 8  2.5  3.0
 8 ≤ t < 15  2.5  3.0
 15 ≤ t < 20
 2.5  3.0
 t 20
 3.0  3.5
  C  t < 8  3.0  3.5
 8 ≤ t < 15  3.0  3.5
 15 ≤ t < 20
 3.0  3.5
 t 20
 3.5  4.0
 D  t < 8  3.5  4.0
 8 ≤ t < 15  4.0  4.5

1) R/t stands for punch radius (R) divided by sheet thickness (t). The guaranteed values are valid under conditions given in the brochure Bending of High Strength Steel.
2) The plate rolling direction.