ABS Grade AH36, DH36, EH36 Z25

Download data sheet

Select Language

Get datasheet by email
Close

Get datasheet by email

    Show specs in Imperial Metric

    General Product Description

    ABS Grades AH36, DH36, and EH36 Z25 are "Z" quality, higher-strength structural steels with a minimum specified yield strength of 51 ksi and specified minimum Charpy V-notch impact toughness properties. The Z25 quality steel has a minimum specified average value for reduction of area in through thickness tensile testing of 25%.

    Applications

    Typical applications include shipbuilding and mobile offshore drilling units and structural details for which greater resistance to lamellar tearing is desired

    Available Dimensions

    Hide/Show specific columns Edit
    Select columns to display
      Grade Product type Thickness
      (inchesmm)
      Width 1)
      (inchesmm)
      Length 1)
      (inchesmm)
      Grade AH36Z25 Plate 0.1875 - 5.904.762 - 150 72 - 129.91800 - 3299 79 - 5902000 - 15000
      Grade DH36Z25 Plate 0.1875 - 5.904.762 - 150 72 - 129.91800 - 3299 79 - 5902000 - 15000
      Grade EH36Z25 Plate 0.1875 - 5.904.762 - 150 72 - 129.91800 - 3299 79 - 5902000 - 15000
      Compare parameters

      Select one parameter to compare

      Comparison

        1) Please inquire for plate dimensions outside the noted range.

        Mechanical Properties

        Tensile testing is performed in the transverse direction. When "Z" quality steel is specified, through-thickness tension testing is performed in accordance with ABS Rules.

        Hide/Show specific columns Edit
        Select columns to display
          Grade Product type Thickness
          (inchesmm)
          Yield strength
          (min ksi)
          Tensile strength
          (ksi)
          Elongation A5 1)
          (min %)
          Reduction of area, average
          (min %)
          Reduction of area
          (min %)
          Grade AH36Z25 Plate 0.1875 - 5.904.762 - 150 51 71 - 90 22 25 15
          Grade DH36Z25 Plate 0.1875 - 5.904.762 - 150 51 71 - 90 22 25 15
          Grade EH36Z25 Plate 0.1875 - 5.904.762 - 150 51 71 - 90 22 25 15
          Compare parameters

          Select one parameter to compare

          Comparison

            1) See ABS Rules for elongation requirements for alternative tensile specimens.

            Impact Properties

            Hide/Show specific columns Edit
            Select columns to display
              Grade Thickness
              (inchesmm)
              Test temperature
              (°F)
              Min Longitudinal Average Energy 1)
              (ft-lbs)
              Min transverse average energy 1)
              (ft-lbs)
              AH36Z25 0.1875 - 2.004.762 - 50.8 32 25 17
              AH36Z25 2.001 - 2.8050.83 - 71.1 32 30 20
              AH36Z25 2.801 - 4.0071.15 - 102 32 37 25
              AH36Z25 4.001 - 5.90101.6 - 150 32 37 25
              DH36Z25 0.1875 - 2.004.762 - 50.8 -4 25 17
              DH36Z25 2.001 - 2.8050.83 - 71.1 -4 30 20
              DH36Z25 2.801 - 4.0071.15 - 102 -4 37 25
              DH36Z25 4.001 - 5.90101.6 - 150 -4 37 25
              EH36Z25 0.1875 - 2.004.762 - 50.8 -40 25 17
              EH36Z25 2.001 - 2.8050.83 - 71.1 -40 30 20
              EH36Z25 2.801 - 4.0071.15 - 102 -40 37 25
              EH36Z25 4.001 - 5.90101.6 - 150 -40 37 25
              Compare parameters

              Select one parameter to compare

              Comparison

                1) Specimen orientation at the option of the manufacturer unless otherwise specified in the order.

                No more than one value below the specified miniminum average energy but no less than 70% of the specfied minimum average energy value.

                Minimum average energy for full-size specimens. Refer to ABS Rules for sub-size specimen energy requirements.

                Carbon Equivalent CET(CEV)

                Hide/Show specific columns Edit
                Select columns to display
                  Grade AH36 DH36 EH36
                  Thickness (inchesmm) 0.1875 - 1.574.762 - 39.9 0.1875 - 1.574.762 - 39.9 0.1875 - 1.574.762 - 39.9
                  CEV 1) (max %) 0.38 0.38 0.38
                  Compare parameters

                  Select one parameter to compare

                  Comparison

                    1) Carbon equivalent requirements for TMCP condition of supply only.