SSAB AM Tough is a gas atomized advanced high strength steel powder for additive manufacturing. SSAB AM Tough is in particular suited in L-PBF (Laser-Powder Bed Fusion) and DED or LMD (Direct Energy Deposition or Laser Metal Deposition).

SSAB AM Tough is targeted towards additive manufacturing of high strength engineering components, heavy machinery, automotive and energy sector where toughness is the most desired property.

 

SSAB AM Tough is available on request as fossil-free steel powder.

Powder Properties

Standard particle size distribution.

L-PBF

20 - 53 µm

DED

53 - 150 µm

Measurement of particle size distribution is according to ISO 13322-2 (Dynamic image analysis methods).

Other particle size distributions can be arranged upon agreement.

Generic Data

Achievable generic data in as-built parts: L-PBF

Density

7.8 g/cm3

Young´s Modulus

235 GPa

 

Mechanical Properties

Achievable mechanical properties in as-built parts: L-PBF

Product
Product
SSAB AM Tough
Hardness
(HV5)
280
Tensile strength
(MPa)
1030
Yield strength
(MPa)
950
Elongation A5
(%)
16
Impact toughness
(Charpy V)
at RT 1)/ at -40 oC
220 J / 80 J

1) At room temperature.

All test samples have been produced on a SLM 280 2.0 system, 30 µm layer thickness and tested in the vertical direction.

Typical Chemical Composition

C
(%)
C
(%)
0.18
Si
(%)
0.23
Mn
(%)
1.09
Nb
(%)
0.013
B
(%)
0.0017
Fe
Balance

 

Delivery Conditions

Standard package size for SSAB AM powder is 10 kg, including silica gel bag. Other package sizes are available up on agreement.

 

Safety Information Sheet

Fossil-free steel

The steel in this product is a proof of concept and pilot delivery of the fossil-free steel SSAB is developing. By using hydrogen reduced sponge iron, SSAB has removed the primary source of CO2 emissions in the steelmaking, emitting water instead of carbon dioxide. Discover more at www.ssab.com.