SSAB M43 is a micro-alloyed steel grade for quench hardening. The self-tempering properties prevent formation of hardening cracks. The degree of hardness and toughness that can be achieved after heat-treatment will provide end products with a wear- and shock resistance ratio that ensures longer lifetime.

Dimension Range

Hide/Show specific columns Edit
Select columns to display
    Delivery form Thickness
    (mmin)
    Width
    (mmin)
    Length
    (mmin)
    Hot rolled sheet 3.0 - 12.0 1)0.12 - 0.472 1) 1000 - 180039.37 - 70.87 - 13000- 511.81
    Compare parameters

    Select one parameter to compare

    Comparison

      1) Please check thickness/width combinations available.

      Mechanical Properties (typical values)

      Hide/Show specific columns Edit
      Select columns to display
        Product type Typical yield strength Rp0.2 (MPa) Typical tensile strength Rm (MPa) Typical Elongation A (%),
        not guaranteed
        Typical Hardness
        (HRC), not guaranteed
        As rolled 440 660 16 18
        Water quenched 2200 58
        Water quenched and tempered (175° C) 56
        Oil quenched 1750 52
        Oil quenched and tempered (175° C) 51
        Compare parameters

        Select one parameter to compare

        Comparison

          Bending radius

          For further information, please consult your local SSAB contact person or contact SSAB’s Technical Customer Service.

          Material Testing

          A material test certificate Type 2.2 according to EN 10204 (chemical composition) is part of the delivery. A material test certificate according Type 3.1 according to EN 10204 (mechanical properties) can be provided by special agreement.

          Impact Properties (typical values)

          Hide/Show specific columns Edit
          Select columns to display
            Product condition Longitudinal test, typical impact energy,
            Charpy V 10x10 mm test specimen 1)
            As rolled / 20.0 °C
            Water quenched 25 J / 20.0 °C
            Water quenched and tempered (175° C) 37 J / 20.0 °C
            Oil quenched 38 J / 20.0 °C
            Oil quenched and tempered (175° C) 39 J / 20.0 °C
            Compare parameters

            Select one parameter to compare

            Comparison

              Product condition
              As rolled
              Longitudinal test, typical impact energy,
              Charpy V 10x10 mm test specimen 1)
              / 20.0 °C
              Product condition
              Water quenched
              Longitudinal test, typical impact energy,
              Charpy V 10x10 mm test specimen 1)
              25 J / 20.0 °C
              Product condition
              Water quenched and tempered (175° C)
              Longitudinal test, typical impact energy,
              Charpy V 10x10 mm test specimen 1)
              37 J / 20.0 °C
              Product condition
              Oil quenched
              Longitudinal test, typical impact energy,
              Charpy V 10x10 mm test specimen 1)
              38 J / 20.0 °C
              Product condition
              Oil quenched and tempered (175° C)
              Longitudinal test, typical impact energy,
              Charpy V 10x10 mm test specimen 1)
              39 J / 20.0 °C

              1) For thicknesses between 6 - 11.9 mm, sub-size Charpy V-specimens are used. The specified typical value is then proportional to the cross-sectional area of the specimen compared to a full-size specimen (10 x 10 mm).

              Chemical Composition (ladle analysis)

              Hide/Show specific columns Edit
              Select columns to display
                C
                (%)
                Si
                (%)
                Mn
                (%)
                S
                (max %)
                P
                (max %)
                Cr
                (max %)
                0.39 - 0.47 0.13 - 0.23 0.20 - 0.30 0.010 0.020 0.10
                Compare parameters

                Select one parameter to compare

                Comparison

                  SSAB M43 is micro-alloyed with Nb, Ti and V.

                  Carbon Equivalent

                  Hide/Show specific columns Edit
                  Select columns to display
                    Delivery form Hot rolled strip
                    Typical CET (%) 0.53
                    Compare parameters

                    Select one parameter to compare

                    Comparison

                      Delivery form
                      Typical CET (%)
                      Hot rolled strip
                      0.53
                      CET and CEV formula

                      Tolerances

                      SSAB M43 is delivered with SSAB tolerances, which meet and exceed the requirements in EN 10051. Tighter tolerances are available upon request

                      Thickness

                      2/3 of EN 10051.

                      Width

                      Hot rolled sheet: -0/+20mm (trimmed edges -0/+2 mm).

                      Length

                      -0/+20mm (only available for cut to length sheets).

                      Shape

                      Tolerances according to EN 10051.

                      Flatness

                      ≤ 6 mm/1 m ruler deviation (only valid for cut to length sheets).

                      Surface Properties

                      According to EN 10163-2 Class A, Subclass 3.

                      Delivery Conditions

                      Hot rolled sheets are delivered in as rolled (+AR) condition.

                      Surface Condition

                      Hot rolled sheets are available in non-pickled, pickled dry or pickled & oiled condition.

                      Fabrication and Other Recommendations

                      Cutting is recommended by laser or plasma.

                      The material is well-suited for welding in as rolled condition, please contact tech support for guidance.

                      For information concerning fabrication, see SSAB´s brochures on www.ssab.com or consult Tech Support.